Preparation method of intermediate-temperature-cured high-bonding-strength epoxy adhesive film
By using a combination of liquid epoxy resin, solid epoxy resin, solid toughener and latent curing agent, the problem of crosslinking of thermosetting films during processing is solved, and excellent adhesive over a wide temperature range is achieved The junction strength and fatigue resistance are suitable for structural bonding of various materials and reduce costs.
Patent Information
- Application Number
- CN202410936286.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-26
AI Technical Summary
The inevitable crosslinking of existing thermosetting films during processing results in damage to adhesive properties, and it is difficult to provide excellent bonding strength in a wide temperature range from ultra-low temperature to normal temperature, which is costly and unsuitable for various materials. structural bonding.
Using epoxy adhesives containing liquid epoxy resin, solid epoxy resin, solid toughener and latent curing agent, avoid crosslinking through specific components mixing and processing methods, ensuring curing at temperatures above 120°C , thereby providing excellent bonding strength and fatigue resistance in ultra-low temperature to normal temperature range.
Excellent bonding strength and fatigue resistance over a wide temperature range are achieved, cost is reduced, and structural bonding of various materials is suitable, avoiding the crosslinking problem of the adhesive film during processing.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to an epoxy adhesive and an epoxy film comprising the epoxy adhesive, and a method for preparing the epoxy film. Background Art
[0002] Epoxy film has excellent structural bonding performance and durable reliability, and is easy to operate as a single component with uniform adhesive application. It is widely used in the bonding of honeycomb sandwich structures in aerospace, rail transit, ships, etc.
[0003] With the development of civil aviation, rail transit, shipbuilding and construction, epoxy resin adhesives are required to have excellent bonding strength at low temperature, room temperature and over-temperature. It is expected that epoxy resins are low in cost, and their flexibility, tensile shear strength, elasticity and fatigue resistance are satisfactory, and they are suitable for structural bonding of various metal and non-metal materials. Adhesives used for bonding panels in honeycomb structures and in honeycomb core materials need to have sufficient bonding strength at room temperature and medium temperature, and must have a thermal expansion coefficient that matches well with different bonded materials. In terms of bonding technology, the adhesive is required to be easy to use, accurately apply glue, and facilitate rapid assembly and production.
[0004] Liquid adhesives need to be prepared before use and tend to flow during bonding, resulting in loss of adhesive and pollution of the working environment. Therefore, solid film form is the preferred adhesive for bonding honeycomb core materials and panels.
[0005] Adhesive film is a type of hot melt adhesive, and its full name is film-like hot melt adhesive. The hot melt adhesive is extruded into a film (sheet) and then rolled into a roll, which is the product. When using the adhesive film, cut the film into the required size and sandwich it between the substrates, and then heat press it to achieve the purpose of bonding.
[0006] The main components of adhesive films are thermoplastic polymer materials and semi-solid adhesives made by blending / polymerization modification. Examples of adhesive films include thermosetting adhesive films and hot melt adhesive films.
[0007] When the adhesive film is heated, it melts into a viscous state and wets the processing surface. When the thermosetting type is further heated, a cross-linking reaction occurs in the thermosetting adhesive film, and the bonding between the materials is achieved through solidification. After the hot-melt adhesive film is separated from the heat source, it cools down and solidifies in a very short time, forming an adhesive layer with a certain strength.
[0008] However, there are defects in the manufacturing process of thermosetting adhesive films. For example, the adhesive films in the prior art are inevitably cross-linked during the processing, resulting in the damage of the adhesive properties of the product film, and even the inability to process the film products suitable for the application.
[0009] Therefore, there is still an urgent need in the art to develop a novel thermosetting adhesive film that can overcome the defects in the prior art and provide excellent bonding strength in a wide temperature range from ultra-low temperature to room temperature, with low cost, satisfactory flexibility, tensile shear strength, elasticity and fatigue resistance, and is suitable for structural bonding of various types of metal and non-metal materials. Summary of the invention
[0010] The purpose of the present application is to provide an adhesive film that can avoid the risk of slow polymerization during film processing and cures at a temperature above 120° C. The adhesive film provides excellent bonding strength in a wide temperature range from ultra-low temperature to room temperature, is low in cost, and has satisfactory flexibility, tensile shear strength, elasticity and fatigue resistance, and is suitable for structural bonding of various types of metal and non-metal materials, and can be used in particular for bonding and sealing between materials with different expansion coefficients.
[0011] A first aspect of the present application relates to an epoxy adhesive, the epoxy adhesive comprising:
[0012] a) a liquid epoxy resin, wherein the liquid epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, brominated bisphenol A epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, alicyclic epoxy resin, or a mixture thereof;
[0013] b) solid epoxy resin;
[0014] c) a solid toughening agent, wherein the solid toughening agent is selected from: styrene-butadiene rubber, MBS resin, ethylene-based terpolymer, or a mixture thereof;
[0015] d) a latent curing agent, wherein the latent curing agent is selected from dicyandiamide, organic urea, modified amine, or a mixture thereof.
[0016] The second aspect of the present application relates to an epoxy film, which comprises:
[0017] - a layer of epoxy adhesive; and
[0018] - a release film layer, wherein the epoxy adhesive comprises:
[0019] a) a liquid epoxy resin, wherein the liquid epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, brominated bisphenol A epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, alicyclic epoxy resin, or a mixture thereof;
[0020] b) solid epoxy resin;
[0021] c) a solid toughening agent, wherein the solid toughening agent is selected from: styrene-butadiene rubber, MBS resin, ethylene-based terpolymer, or a mixture thereof;
[0022] d) a latent curing agent, wherein the latent curing agent is selected from dicyandiamide, organic urea, modified amine, or a mixture thereof.
[0023] The third aspect of the present application relates to a method for preparing the adhesive film according to the second aspect of the present application, the method comprising the following steps:
[0024] 1) Mix the following components:
[0025] a) a liquid epoxy resin, wherein the liquid epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, brominated bisphenol A epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, alicyclic epoxy resin, or a mixture thereof;
[0026] b) a solid epoxy resin, wherein the solid epoxy resin is in a solid state at room temperature;
[0027] c) a solid toughening agent, wherein the solid toughening agent is selected from: styrene-butadiene rubber, MBS resin, ethylene-based terpolymer, or a mixture thereof;
[0028] d) a latent curing agent, wherein the latent curing agent is selected from dicyandiamide, organic urea, modified amine, or a mixture thereof;
[0029] 2) applying the mixture obtained in step 1) on a first release film to form an adhesive film, wherein the first surface of the epoxy adhesive layer is in contact with the first release film;
[0030] 3) Optionally, a second release film layer is covered on the second surface of the epoxy adhesive layer.
[0031] A fourth aspect of the present application relates to a method for bonding different materials, the method comprising the following steps:
[0032] 1) Applying an epoxy adhesive comprising:
[0033] a) a liquid epoxy resin, wherein the liquid epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, brominated bisphenol A epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, alicyclic epoxy resin, or a mixture thereof;
[0034] b) solid epoxy resin;
[0035] c) a solid toughening agent, wherein the solid toughening agent is selected from: styrene-butadiene rubber, MBS resin, ethylene-based terpolymer, or a mixture thereof;
[0036] d) a latent curing agent, wherein the latent curing agent is selected from dicyandiamide, organic urea, modified amine, or a mixture thereof;
[0037] 2) contacting the second substrate with the surface of the first substrate with the adhesive to obtain a first laminate;
[0038] 3) subjecting the first laminate to curing at a curing temperature greater than or equal to 120°C.
[0039] The applicant has unexpectedly discovered that, through the combination of components a) to d) of the first aspect of the present application, the adhesive can be made not to undergo crosslinking during the process of being formed into a film, and can produce satisfactory bonding after the adhesive is cured at a temperature above 120°C, and such bonding provides excellent bonding strength over a wide temperature range (e.g., -196 to 100°C). DETAILED DESCRIPTION
[0040] "Scope" disclosed herein is defined in the form of lower limit and upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a particular range. The scope defined in this way can be inclusive or exclusive of end values, and can be arbitrarily combined, i.e., any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following range can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In this application, unless otherwise specified, the numerical range "a to b" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0 to 5" means that all real numbers between "0 to 5" are listed in this document, and "0 to 5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0041] In this application, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution.
[0042] In this application, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.
[0043] In the present application, unless otherwise specified, all steps mentioned herein may be performed sequentially or randomly, but are preferably performed sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0044] In this application, unless otherwise specified, the terms "include" and "comprising" mentioned herein may be open-ended or closed-ended. For example, the terms "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0045] In the description of this article, it should be noted that, unless otherwise specified, "above" and "below" are inclusive of the number itself, and "several" in "one or several" means two or more.
[0046] In the description herein, unless otherwise specified, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0047] Herein, unless otherwise specified, percentage (%) or part refers to percentage by weight or part by weight relative to the composition.
[0048] Herein, if there is no contrary description, the sum of the contents of the various components in the composition is 100%.
[0049] Herein, if there is no contrary description, the sum of the parts of each component in the composition may be 100 parts by weight.
[0050] In this document, unless otherwise specified, "a combination thereof" means a multi-component mixture of the elements described, for example a mixture of two, three, four and up to the maximum possible multi-component mixture.
[0051] If not specifically stated, the terms "a" or "an" used in the present specification means "at least one".
[0052] Herein, unless otherwise stated, all reactions are carried out at normal temperature and pressure.
[0053] In the present application, unless otherwise specified, all terms "parts" refer to parts by weight.
[0054] A first aspect of the present application relates to an epoxy adhesive, the epoxy adhesive comprising:
[0055] a) a liquid epoxy resin, wherein the liquid epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, brominated bisphenol A epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, alicyclic epoxy resin, or a mixture thereof;
[0056] b) solid epoxy resin;
[0057] c) a solid toughening agent, wherein the solid toughening agent is selected from: styrene-butadiene rubber, MBS resin, ethylene-based terpolymer, or a mixture thereof;
[0058] d) a latent curing agent, wherein the latent curing agent is selected from dicyandiamide, organic urea, modified amine, or a mixture thereof.
[0059] Liquid epoxy resin
[0060] In the context of the present application, "liquid epoxy resin" means an epoxy resin that is liquid at normal temperature.
[0061] According to one embodiment, the liquid epoxy resin can be selected from: bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, brominated bisphenol A epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, alicyclic epoxy resin, or a mixture thereof.
[0062] According to a preferred embodiment, the liquid epoxy resin is selected from bisphenol A epoxy resin, bisphenol F epoxy resin, aliphatic glycidyl ether epoxy resin and glycidyl ester epoxy resin or a mixture thereof.
[0063] According to a preferred embodiment, the epoxide equivalent of the liquid epoxy resin is 156 to 2500 g / eq, or 170 to 2200 g / eq, or 200 to 2000 g / eq, or 300 to 1800 g / eq, or 400 to 1700 g / eq, or 500 to 1600 g / eq, or 600 to 1500 g / eq, or 700 to 1200 g / eq, or 800 to 1100 g / eq, or 900 to 1000 g / eq.
[0064] According to a preferred embodiment, the number average molar mass of the liquid epoxy resin is 300 to 500 g / mol, preferably 350 to 500 g / mol, more preferably 400 to 500 g / mol. For example, the molecular weight of the liquid epoxy resin may be 310 g / mol, or 320 g / mol, or 330 g / mol, or 340 g / mol, or 350 g / mol, or 360 g / mol, or 370 g / mol, or 380 g / mol, or 390 g / mol, or 400 g / mol, or 410 g / mol, or 420 g / mol, or 430 g / mol, or 440 g / mol, or 450 g / mol, or 460 g / mol, or 470 g / mol, or 480 g / mol, or 490 g / mol, or 500 g / mol.
[0065] According to a preferred embodiment, the liquid epoxy resin has an average of 2 to 5 epoxy functional groups per molecule, preferably 2.5 to 5 epoxy functional groups, preferably 3 to 5 epoxy functional groups, preferably 3.5 to 5 epoxy functional groups. For example, the liquid epoxy resin has an average of 2, 2.1, or 2.2, or 2.3, or 2.4, or 2.5, or 2.6, or 2.7, or 2.8, or 2.9, or 3.0, or 3.1, or 3.2, or 3.3, or 3.4, or 3.5, or 3.6, or 3.7, or 3.8, or 3.9, or 4.0, or 4.1, or 4.2, or 4.3, or 4.4, or 4.5, or 4.6, or 4.7, or 4.8, or 4.9, or 5 epoxy functional groups per molecule.
[0066] The liquid epoxy resin may be commercially available. As non-limiting examples, the following liquid epoxy resins may be mentioned: bisphenol A type liquid epoxy resin NPEL-127E, bisphenol A type liquid epoxy resin 6101, bisphenol A type liquid epoxy resin 128, bisphenol A type liquid epoxy resin E44, ARALDITE GY250, ARALDITE GY9708-3, ARALDITE MY790-1, ARALDITE CY179-1, ARALDITE CY184, ARALDITE GY6010, ARALDITE GY2600, EPALLOY 5000, EPALLOY 5001LC, NPEF-1, NPEL-127, NPEL-127H, NPEL-127L, NPEL-128, NPEL-12BB, NPEL-128R, NPEL-128s, NPE-1286, NPEL-131, NPEL-144; DER-331 (liquid; epoxy equivalent weight 182 to 192; viscosity at 25°C 11000 to 14000 centipoise) and DER-332 (liquid; epoxy equivalent weight 171 to 175; viscosity at 25°C 4000 to 6000 centipoise) from Olin; available from Hexion Speciality Chemicals EPON828 (liquid; epoxy equivalent weight 185 to 192; viscosity at 25°C 11,000 to 15,000 centipoise), EPON830 (liquid; epoxy equivalent weight 190 to 198; viscosity at 25°C 17,000 to 22,500 centipoise), and EPON1001F (liquid; epoxy equivalent weight: 525 to 550; viscosity at 25°C 7,000 to 9,600 centipoise) from Dainippon Ink and Chemicals, Inc. 830 from Olin (liquid; epoxy equivalent weight 165 to 180; viscosity at 25°C is 3000 to 4000 centipoise); DER-354 from Olin (liquid; epoxy equivalent weight 167 to 174; viscosity at 25°C is 3400 to 4200 centipoise); EPIKOTE 828 from Hexion Speciality Chemicals (Rosbach, Germany) (liquid; epoxy equivalent weight 184 to 190; viscosity at 25°C is 12000 to 14000 centipoise); EPILOX A 18-00 from Leuna Epilox GmbH (Leuna, Germany) (liquid; epoxy equivalent weight 175 to 185; viscosity at 25°C is 8000 to 10000 centipoise).
[0067] In a preferred embodiment, the content of the liquid epoxy resin in the epoxy adhesive of the first aspect of the present application is 30 to 50 parts, preferably 35 to 50 parts, preferably 40 to 50 parts, preferably 45 to 50 parts. For example, the content of the liquid epoxy resin in the epoxy adhesive of the first aspect of the present application may be 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts, 46 parts, 48 parts of liquid epoxy resin.
[0068] Solid epoxy resin
[0069] In the context of the present application, the term "solid epoxy resin" means an epoxy resin that is solid at normal temperature.
[0070] According to a preferred embodiment, the epoxy equivalent of the solid epoxy resin is 450 to 2500 g / eq, or 450 to 1700 g / eq, or 500 to 1600 g / eq, or 600 to 1500 g / eq, or 700 to 1200 g / eq, or 800 to 1100 g / eq, or 900 to 1000 g / eq.
[0071] According to a preferred embodiment, the number average molecular weight of the solid epoxy resin is greater than 1000 g / mol, or greater than 1500 g / mol, or greater than 2000 g / mol, or greater than 2500 g / mol, or greater than 3000 g / mol.
[0072] According to one embodiment, the number average molecular weight of the solid epoxy resin is less than 10000 g / mol, or less than 9000 g / mol, or less than 8000 g / mol, or less than 7000 g / mol, or less than 6000 g / mol, or less than 5000 g / mol.
[0073] For example, the number average molecular weight of the solid epoxy resin may be 1000 g / mol, or 1200 g / mol, or 1400 g / mol, or 1600 g / mol, or 1800 g / mol, or 2000 g / mol, or 2200 g / mol, or 2400 g / mol, or 2600 g / mol, or 2800 g / mol, or 3000 g / mol, or 4000 g / mol.
[0074] According to a preferred embodiment, the solid epoxy resin has an average of 2 to 5 epoxy functional groups per molecule, preferably 2.5 to 5 epoxy functional groups, preferably 3 to 5 epoxy functional groups, preferably 3.5 to 5 epoxy functional groups. For example, the solid epoxy resin has an average of 2.1, or 2.2, or 2.3, or 2.4, or 2.5, or 2.6, or 2.7, or 2.8, or 2.9, or 3.0, or 3.1, or 3.2, or 3.3, or 3.4, or 3.5, or 3.6, or 3.7, or 3.8, or 3.9, or 4.0, or 4.1, or 4.2, or 4.3, or 4.4, or 4.5, or 4.6, or 4.7, or 4.8, or 4.9 epoxy functional groups per molecule.
[0075] According to a preferred embodiment, the solid epoxy resin is selected from: solid bisphenol A epoxy resin, solid bisphenol A novolac epoxy resin, bisphenol S glycidyl ether epoxy resin, glycidyl ester epoxy resin.
[0076] The solid epoxy resin is commercially available. As non-limiting examples, the following solid epoxy resins may be mentioned: ARALDITE GT7071, ARALDITE GT7072, ARALDITE GT7004, ARALDITE GT6084-2, ARALDITE GT6097, ARALDITE GT6099, ARALDITE GT6610, ARALDITE GT7255, ARALDITE GT7013, ARALDITE GT7074, bisphenol A type solid epoxy resin NPES-903, bisphenol A type solid epoxy resin NPES-905L, bisphenol A type solid epoxy resin NPES-904.
[0077] In a preferred embodiment, the solid epoxy resin is selected from isophthalic acid epoxy resin and trimesic acid epoxy resin.
[0078] In a preferred embodiment, in the epoxy adhesive of the first aspect of the present application, the content of solid epoxy resin is 30 to 50 parts, preferably 35 to 50 parts, preferably 40 to 50 parts, preferably 45 to 50 parts. For example, the content of the solid epoxy resin in the epoxy adhesive of the first aspect of the present application may be 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts, 46 parts, 48 parts of solid epoxy resin.
[0079] Solid toughening agent
[0080] In the context of the present application, the term "solid toughening agent" means a toughening agent that is solid at room temperature.
[0081] In one embodiment of the present application, the solid toughening agent may be selected from: styrene-butadiene rubber, MBS resin, ethylene-based terpolymer, or a mixture thereof.
[0082] As non-limiting examples of solid toughening agents suitable for the present application, mention may be made of those commercially available under the name BLD-518 from Shandong Bangtai Petrochemical Co., Ltd., those commercially available under the name SEBS6151 from Nantong Taiwan Rubber Co., Ltd., and those commercially available under the trade name Elvaloy PTW from The Dow Chemical Company.
[0083] In a preferred embodiment, the melting point of the solid toughening agent is lower than 200° C., preferably lower than 190° C., preferably lower than 180° C., preferably lower than 170° C. For example, the melting point of the solid toughening agent may be about 80° C., or about 85° C., or about 90° C., or about 95° C., or about 100° C., or about 105° C., or about 110° C., or about 115° C., or about 120° C., or about 125° C., or about 130° C., or about 135° C., or about 140° C., or about 145° C., or about 150° C., or about 155° C., or about 160° C., or about 165° C., or about 170° C., or about 175° C., or about 180° C., or about 185° C., or about 190° C., or about 195° C.
[0084] In the epoxy adhesive of the first aspect of the present application, the content of the solid toughening agent is not particularly limited, and the content of the solid toughening agent may depend on the desired quality of the final product.
[0085] In one embodiment, the solid toughening agent content in the epoxy adhesive of the first aspect of the present application is 0.1 to 5 parts, preferably 1.5 to 3.5 parts, preferably 2.5 to 3 parts. For example, the solid toughening agent content in the epoxy adhesive of the first aspect of the present application may be 0.2 parts, or 0.4 parts, or 0.6 parts, or 0.8 parts, or 1 parts, or 1.2 parts, or 1.4 parts, or 1.6 parts, or 1.8 parts, or 2 parts, or 2.2 parts, or 2.4 parts, or 2.6 parts, or 2.8 parts, or 3 parts, or 3.2 parts, or 3.4 parts, or 3.6 parts, or 3.8 parts, or 4 parts, or 4.2 parts, or 4.4 parts, or 4.6 parts, or 4.8 parts.
[0086] Latent curing agent
[0087] In the context of the present application, the term "latent curing agent" means a curing agent that, after being added to an epoxy resin, forms a single-component system with the epoxy resin having a certain storage stability at room temperature, and can rapidly undergo a curing reaction under conditions of heating, light, moisture, pressure, etc. For example, the latent curing agent and the epoxy resin can rapidly undergo a curing reaction under heating conditions.
[0088] In an illustrative but non-limiting example, the latent curing agent may prevent the crosslinking reaction of the epoxy resin from occurring at 100° C. However, it should be understood that the present application is by no means limited thereto.
[0089] In one embodiment, the latent curing agent may be selected from dicyandiamide, organic urea, modified amine, or a mixture thereof.
[0090] The latent curing agent may be commercially available. As non-limiting examples, the following brands of latent curing agents may be mentioned: ARADUR2844, ARADUR3380-1, ARADUR835, ARADUR9690-1, ARADUR9506, ARADUR5200, and ARADURDY9577.
[0091] In the epoxy adhesive of the first aspect of the present application, the content of the latent curing agent is not particularly limited, and the content of the latent curing agent may depend on the desired quality of the final product.
[0092] In one embodiment, in the epoxy adhesive of the first aspect of the present application, the content of the latent curing agent is 5 to 15 parts, preferably 7 to 13 parts, preferably 9 to 11 parts. For example, the content of the latent curing agent in the epoxy adhesive of the first aspect of the present application may be 6 parts, or 7 parts, or 8 parts, or 9 parts, or 10 parts, or 11 parts, or 12 parts, or 13 parts, or 14 parts of latent curing agent.
[0093] Liquid toughening agent
[0094] According to a preferred embodiment, the epoxy adhesive of the first aspect of the present application further comprises: e) a liquid toughening agent.
[0095] In the context of the present application, the term "liquid toughening agent" refers to a toughening agent that is liquid at room temperature.
[0096] According to a preferred embodiment, the liquid toughening agent is selected from liquid nitrile rubber, liquid polysulfide rubber, polyether active toughening agent, rubber modified epoxy resin, polyurethane modified epoxy resin, or a combination thereof.
[0097] As non-limiting examples, mention may be made of liquid toughening agents of the following brands: liquid nitrile rubbers such as HyPox 1300*8, HyPox 1300*13; carboxyl-terminated nitrile rubbers such as CTBN 1300X8, CTBN 1300X13, CTBN 1300X18, CTBN 1300X31; amine-terminated nitrile rubbers such as ATBN 1300X21, ATBN 1300X16, ATBN 1300X16, ATBN1300X, ATBN 1300X35, ATBN 1300X42; terminal nitrile rubbers such as VTBN 1300X33LC, VTBN1300X43LC, VTB 2000X168; epoxy-terminated nitrile rubbers such as ETBN 1300X40, ETBN 1300X68, ETBN1300X63, ETB 2000X174; hydroxyl-terminated liquid polybutadiene such as HTB; rubber-modified epoxy resin such as MX154, MX158; polyurethane-modified epoxy resin such as SL3451~SL3453.
[0098] Mention may also be made, as non-limiting examples, of liquid toughening agents commercially available from Shanghai Huayi Resin Co., Ltd. under the grades 3001, 3002, 801340, 901350, RN55.
[0099] The content of the liquid toughening agent depends on the desired product properties. As a non-limiting example, the content of the liquid toughening agent in the epoxy adhesive of the first aspect of the present application is 10 to 15 parts, such as 11 parts, or 12 parts, or 13 parts, or 14 parts.
[0100] Curing accelerator
[0101] According to a preferred embodiment, the epoxy adhesive of the first aspect of the present application further comprises: f) a curing accelerator.
[0102] In the context of the present application, the term "curing accelerator" means a substance added to accelerate the reaction rate of epoxy resin and curing agent to reduce the curing reaction temperature and shorten the curing time.
[0103] The curing accelerator is not particularly limited. In an exemplary embodiment, the curing accelerator may be selected from: imidazole and its derivatives, and amine adducts.
[0104] For example, the curing accelerator may be imidazole, 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, an adduct of 2-methylimidazole and butyl glycidyl ether, or an adduct of 2-methylimidazole and 2-ethylhexyl glycidyl ether.
[0105] The curing accelerator may be, for example, those available under the brand name Dyhard (eg, Dyhard UR500, Dyhard UR300), or those available from Ajinomoto Co., Ltd. under the brand name PN (eg, PN-23), or those available under the brand name MY (eg, MY-24), but are by no means limited thereto.
[0106] The amount of the curing accelerator may depend on the desired final product properties. For example, the amount of the curing accelerator in the epoxy adhesive of the first aspect of the present application may be 1 to 10 parts, preferably 2 to 9 parts, preferably 3 to 8 parts, preferably 4 to 7 parts, preferably 5 to 6 parts.
[0107] Additives
[0108] According to a preferred embodiment, the epoxy adhesive of the first aspect of the present application further comprises: g) an auxiliary agent.
[0109] In the context of the present application, the term "auxiliary agent" means a chemical added in addition to components a) to f) for improving the properties or processing of epoxy resins.
[0110] As non-limiting examples, the auxiliary agents that may be mentioned include: inorganic fillers, pigments, system stabilizers, tackifiers, impact modifiers, defoamers, coupling agents, diluents, anti-aging agents.
[0111] According to one embodiment, the inorganic filler may be selected from aluminum hydroxide particles, silicon dioxide particles, calcium carbonate particles, aluminum oxide particles, and the like.
[0112] According to one embodiment, the pigment may be titanium dioxide, carbon black, or the like.
[0113] According to one embodiment, the system stabilizer may be selected from one or more of thiourea, hydroquinone, methoxyphenol and 2,6-di-tert-butyl-p-cresol.
[0114] According to one embodiment, the tackifier may be an acrylic copolymer tackifier, such as acResin DS 3532 from BASF; P-2M (2-hydroxyethyl methacrylate phosphate) from KYOEISHA CHEMICAL.
[0115] The impact modifier may be commercially available, for example, MBS (methacrylate-butadiene-styrene) core-shell copolymer impact modifier produced by Dow, with an average particle size of 100 to 400 microns; NBR (butadiene-acrylonitrile rubber) impact modifier produced by ARLANXEO HighPerformance, with an average particle size of 500 to 900 microns.
[0116] The auxiliary agent is not particularly limited. In an exemplary embodiment, the auxiliary agent is selected from a defoaming agent and a silane coupling agent.
[0117] As examples of defoamers, mention may be made of those available under the following trade names: BYK-W903, BYK-W909, BYK-W920, BYK-W935, BYK-W940, BYK-A535, BYK-052, BYK-052, BYK-088, BYK-077, BYK-071, BYK-070, BYK-065, BYK-A500, BYK-A525, BYK-055, BYK-141, BYK-A530, BYK-054, BYK-S 732 and BYK-A506.
[0118] According to one embodiment, the coupling agent is a silane coupling agent. As examples of silane coupling agents, there can be mentioned KH550, KH 560, KH 570, SCA A10E, SCA A10M, SCA E87F, SCA E87T, etc.
[0119] The amount of the auxiliary agent may depend on the desired final product properties. In an exemplary embodiment, the content of the auxiliary agent in the epoxy adhesive of the first aspect of the present application may be 1 to 3 parts, such as 1.2 parts, or 1.4 parts, or 1.6 parts, or 1.8 parts, or 2.0 parts, or 2.2 parts, or 2.4 parts, or 2.6 parts, or 2.8 parts.
[0120] It should be understood that the examples listed in the present application are merely illustrative examples and do not limit the present application in any way.
[0121] A second aspect of the present application provides an epoxy film, the epoxy film comprising:
[0122] - a layer of epoxy adhesive; and
[0123] - a release film layer, wherein the epoxy adhesive comprises:
[0124] a) a liquid epoxy resin, wherein the liquid epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, brominated bisphenol A epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, alicyclic epoxy resin, or a mixture thereof;
[0125] b) solid epoxy resin;
[0126] c) a solid toughening agent, wherein the solid toughening agent is selected from: styrene-butadiene rubber, MBS resin, ethylene-based terpolymer, or a mixture thereof;
[0127] d) a latent curing agent, wherein the latent curing agent is selected from dicyandiamide, organic urea, modified amine, or a mixture thereof.
[0128] In an embodiment of the present application, the release film layer may be applied on one side or both sides of the epoxy adhesive layer.
[0129] The release film layer can be made of any suitable material. For example, the material of the release film can be PE, PET, OPP, PC, PS, PMMA, BOPP, TPX, PVC, PTFE, silicone oil paper, etc. Preferably, the release film is PE or silicone oil paper.
[0130] In the epoxy adhesive layer, the epoxy adhesive is as described in the first aspect of the present application.
[0131] In a preferred embodiment, the epoxy adhesive in the epoxy film of the second aspect of the present application may include one or more of the following further components: e) a liquid toughening agent, f) a curing accelerator, g) an auxiliary agent. Components a) to g) are all as described in the first aspect of the present application.
[0132] The third aspect of the present application provides a method for preparing the adhesive film according to the second aspect of the present application, the method comprising the following steps:
[0133] 1) Mix the following components:
[0134] a) a liquid epoxy resin, wherein the liquid epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, brominated bisphenol A epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, alicyclic epoxy resin, or a mixture thereof;
[0135] b) a solid epoxy resin, wherein the solid epoxy resin is in a solid state at room temperature;
[0136] c) a solid toughening agent, wherein the solid toughening agent is selected from: styrene-butadiene rubber, MBS resin, ethylene-based terpolymer, or a mixture thereof;
[0137] d) a latent curing agent, wherein the latent curing agent is selected from dicyandiamide, organic urea, modified amine, or a mixture thereof;
[0138] 2) applying the mixture obtained in step 1) on a first release film to form an adhesive film, wherein the first surface of the epoxy adhesive layer is in contact with the first release film;
[0139] 3) Optionally, a second release film layer is covered on the second surface of the epoxy adhesive layer.
[0140] According to a preferred embodiment, step 1) comprises mixing one or more of the following further components with components a) to d): e) a liquid toughening agent, f) a curing accelerator, g) an auxiliary agent. Components a) to g) are all as described in the first aspect of the present application.
[0141] The application method in step 2) may be a method well known to those skilled in the art. As examples of the application method in step 2), coating (e.g., blade coating, spin coating, roller coating), thermoforming (e.g., calendering, hot pressing, stretching, extrusion), casting, etc. may be mentioned, but the application methods that can be used in the present application are not limited thereto.
[0142] In a preferred embodiment, step 2) of the third aspect of the present application includes the following sub-steps:
[0143] 2-1) Rolling the mixture obtained in step 1) into a film at a temperature T1 using a first rotation speed
[0144] 2-2) Covering the calendered first surface with a release film layer.
[0145] In a preferred embodiment, the temperature T1 is 60 to 85°C, for example, 62°C, 64°C, 66°C, 68°C, 70°C, 72°C, 74°C, 76°C, 78°C, 80°C, 81°C, 82°C, 83°C, 84°C.
[0146] The first rotating speed can be selected as required. As a non-limiting example, a rotating speed of 10 to 120 rpm, or a rotating speed of 40 to 100 rpm can be used. For example, a rotating speed of 20 rpm, or 30 rpm, or 40 rpm, or 50 rpm, or 60 rpm, or 70 rpm, or 80 rpm, or 90 rpm, or 100 rpm, or 110 rpm can be used.
[0147] In another embodiment, step 2) of the third aspect of the present application includes the following sub-steps:
[0148] 2-1) allowing the mixture obtained in step 1) to flow at a temperature T2,
[0149] 2-2) The flowing mixture in 2-1) is cast.
[0150] In a preferred embodiment, the temperature T2 is 60 to 85°C, for example, 62°C, 64°C, 66°C, 68°C, 70°C, 72°C, 74°C, 76°C, 78°C, 80°C, 81°C, 82°C, 83°C, 84°C.
[0151] A fourth aspect of the present application relates to a method for bonding different materials, the method comprising the following steps:
[0152] An epoxy adhesive comprising:
[0153] a) a liquid epoxy resin, wherein the liquid epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, brominated bisphenol A epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, alicyclic epoxy resin, or a mixture thereof;
[0154] b) solid epoxy resin;
[0155] c) a solid toughening agent, wherein the solid toughening agent is selected from: styrene-butadiene rubber, MBS resin, ethylene-based terpolymer, or a mixture thereof;
[0156] d) a latent curing agent, wherein the latent curing agent is selected from dicyandiamide, organic urea, modified amine, or a mixture thereof;
[0157] 2) contacting the second substrate with the surface of the first substrate with the adhesive to obtain a first laminate;
[0158] 3) subjecting the first laminate to curing at a curing temperature greater than or equal to 120°C.
[0159] The application method in step 1) of the fourth aspect is well known to those skilled in the art. In an exemplary embodiment, the application method is blade coating, spin coating, roller coating, drum coating, or drop coating.
[0160] In a preferred embodiment, step 1) of the fourth aspect of the present application comprises mixing one or more of the following further components with components a) to d): e) a liquid toughening agent, f) a curing accelerator, g) an auxiliary agent. Components a) to g) are all as described in the first aspect of the present application.
[0161] In a preferred embodiment, step 1) of the fourth aspect of the present application includes the following sub-steps:
[0162] 1-a) mixing the components of the epoxy adhesive;
[0163] 1-b) Applying the mixture obtained in substep 1-a) directly onto a first substrate.
[0164] In another preferred embodiment, step 1) of the fourth aspect of the present application includes the following sub-steps:
[0165] 1-1) preparing the adhesive film as described in the second aspect of the present application or the adhesive film prepared by the method described in the third aspect of the present application; and
[0166] 1-2) applying the adhesive layer in the adhesive film onto the first substrate so that the first surface of the adhesive layer is in contact with the first substrate.
[0167] Sub-step 1-2) can be performed by means known to those skilled in the art.
[0168] In an exemplary embodiment, step 2) comprises the following sub-steps:
[0169] -Cut the film to the required size,
[0170] - removing the first release film to expose the first surface of the adhesive film;
[0171] - bringing the first surface into contact with a first substrate by applying a certain pressure.
[0172] In a preferred embodiment, step 3) in the fourth aspect of the present application is carried out at a temperature greater than or equal to 120°C and less than 150°C. For example, step 3) can be carried out at 122°C, 124°C, 126°C, 128°C, 130°C, 132°C, 134°C, 136°C, 138°C, 140°C, 142°C, 144°C, 146°C, or 148°C.
[0173] In a preferred embodiment, the duration of step 3) is 1 to 6 hours, for example, 2 hours, 3 hours, 4 hours, or 5 hours.
[0174] The present application is further described below in conjunction with specific examples. It should be understood that the examples provided are only for illustrative purposes and are not intended to limit the present application in any way.
[0175] Example
[0176] The raw materials used in the examples of this application are as follows:
[0177] Liquid Epoxy Resin:
[0178] Bisphenol A liquid epoxy resin NPEL-127E: Nanya Electronic Materials (Kunshan) Co., Ltd.
[0179] Bisphenol A liquid epoxy resin 6101: Shanghai Resin Factory Co., Ltd.
[0180] Bisphenol A liquid epoxy resin 128: Nanya Electronic Materials (Kunshan) Co., Ltd.
[0181] Bisphenol A type liquid epoxy resin E44: Shanghai Resin Factory Co., Ltd.
[0182] XY694 Glycidyl Ether Epoxy Resin: Anhui Xinyuan New Materials Co., Ltd.
[0183] Solid epoxy resin:
[0184] Bisphenol A solid epoxy resin NPES-903: Nanya Electronic Materials (Kunshan) Co., Ltd.
[0185] Bisphenol A solid epoxy resin NPES-905L: Nanya Electronic Materials (Kunshan) Co., Ltd.
[0186] Bisphenol A solid epoxy resin NPES-904: Nanya Electronic Materials (Kunshan) Co., Ltd.
[0187] Solid toughening agent
[0188] MBS: Shandong Bangtai Petrochemical Co., Ltd., BLD-518
[0189] SEBS: Nantong TSRC Co., Ltd., SEBS6151
[0190] Elvaloy PTW: The Dow Chemical Company
[0191] ABS engineering plastic particles: Taiwan Chi Mei Industrial Co., Ltd., PA-757AB
[0192] Liquid toughening agent
[0193] 3001: Shanghai Huayi Resin Co., Ltd.
[0194] 3002: Shanghai Huayi Resin Co., Ltd.
[0195] Latent curing agent
[0196] Dicyandiamide: Azken (Shanghai) Chemical Co., Ltd.
[0197] DDS: India Atu International Trading (Shanghai) Co., Ltd.
[0198] Curing accelerator:
[0199] DyhardUR500: Azken (Shanghai) Chemical Co., Ltd.
[0200] MY-24: Japanese Ajinomoto
[0201] DyhardUR300: Azken (Shanghai) Chemical Co., Ltd.
[0202] Defoaming agent
[0203] BYK A530: BYK Chemical
[0204] Coupling agent
[0205] KH550: Nanjing Aocheng Chemical Co., Ltd.
[0206] Release film:
[0207] PE film, produced by Suzhou Ouchi New Material Technology Co., Ltd.
[0208] Silicone oil paper, Suzhou Jiateng Packaging Material Technology Co., Ltd., JH140HA
[0209] In the present application, the epoxy adhesive is peeled off from the release film after the adhesive film is prepared. If there is no observable residual adhesive on the release film after peeling, it is considered that the epoxy adhesive can be peeled off from the release film. Otherwise, it is considered that the epoxy adhesive cannot be peeled off from the release film.
[0210] In the present application, the method for judging whether the epoxy adhesive is completely cured is as follows: heating at a heating rate of 10°C / min in DSC. If no obvious exothermic signal is observed during the heating process, it means that the epoxy adhesive is completely cured.
[0211] Embodiment 1:
[0212] Prepare the epoxy film by the following steps:
[0213] 1) 40 g of bisphenol A liquid epoxy resin NPEL-127E, 40 g of bisphenol A solid epoxy resin NPES-903, 2 g of MBS resin, and 10 g of toughening agent 3001 were weighed according to mass fraction and added into a planetary mixer, the temperature was controlled at 120° C., and mixed for 2 h to obtain an intermediate.
[0214] 2) Lower the temperature to 80°C, continue to add 8g of latent curing agent dicyandiamide 100s, 5g of curing accelerator DyhardUR500, 2g BYK A530 and 2g KH550 into a planetary mixer, control the temperature below 80°C, mix for 45 minutes, and obtain a rubber compound.
[0215] 3) preheating the adhesive obtained in step 2) at a temperature of 60° C. for 30 min, and then hot-pressing the adhesive on silicone oil paper on an adhesive film making machine at a roller temperature of 80° C. to form a film, wherein the first surface of the epoxy adhesive layer is in contact with the silicone oil paper;
[0216] 4) Cover the second surface of the epoxy adhesive layer with a PE film, roll it into a roll, inspect and package it for storage, and store it in a frozen warehouse.
[0217] Before use, take the film out of the ice storage to restore to room temperature, cut the film into the required size, remove the PE film on the upper surface, press the film to the bonding surface by applying a certain pressure, then remove the silicone paper on the lower surface, overlap it with another adhesive and send it to the oven for curing. Stable bonding can be achieved by heating at 140℃ for 3 hours. After stable bonding, performance testing can be carried out.
[0218] Embodiment 2:
[0219] Prepare the epoxy film by the following steps:
[0220] 1) 30 g of bisphenol A liquid epoxy resin 6101, 40 g of bisphenol A solid epoxy resin NPES-903, 2 g of styrene-butadiene rubber SEPS, and 10 g of toughening agent 3001 were weighed by mass fraction and added into a planetary mixer, the temperature was controlled at 120° C., and mixed for 2 h to obtain an intermediate;
[0221] 2) Lower the temperature to 80°C, continue to add 10g of latent curing agent dicyandiamide for 100s, 6g of curing accelerator MY-24, 2g BYK A530 and 2g KH550 into a planetary mixer, control the temperature below 80°C, mix for 45min, and obtain a rubber compound;
[0222] 3) preheating the adhesive obtained in step 2) at a temperature of 60° C. for 30 min, and then hot-pressing the adhesive on silicone oil paper on an adhesive film making machine at a roller temperature of 80° C. to form a film, wherein the first surface of the epoxy adhesive layer is in contact with the silicone oil paper;
[0223] 4) Cover the second surface of the epoxy adhesive layer with a PE film, roll it into a roll, inspect and package it for storage, and store it in a frozen warehouse.
[0224] Before use, take the film out of the ice storage to restore to room temperature, cut the film into the required size, remove the PE film on the upper surface, press the film to the bonding surface by applying a certain pressure, then remove the silicone paper on the lower surface, overlap it with another adhesive and send it to the oven for curing. Stable bonding can be achieved by heating at 130°C for 3 hours. After stable bonding, performance testing can be carried out.
[0225] Embodiment 3:
[0226] Prepare the epoxy film by the following steps:
[0227] 1) 30 g of bisphenol A liquid epoxy resin 6101, 30 g of bisphenol A solid epoxy resin NPES-905L, 2 g of styrene-butadiene rubber SEPS, and 10 g of toughening agent 3002 were weighed by mass fraction and added into a planetary mixer, the temperature was controlled at 130° C., and mixed for 2 h to obtain an intermediate;
[0228] 2) Lower the temperature to 80°C, continue to add 10g of latent curing agent dicyandiamide for 100s, 8g of curing accelerator MY-24, 2g of BYK A530 and 2g of KH550 into a planetary mixer, control the temperature below 80°C, mix for 45min, and obtain a rubber compound;
[0229] 3) preheating the adhesive obtained in step 2) at a temperature of 60° C. for 30 min, and then hot-pressing the adhesive on silicone oil paper on an adhesive film making machine at a roller temperature of 80° C. to form a film, wherein the first surface of the epoxy adhesive layer is in contact with the silicone oil paper;
[0230] 4) Cover the second surface of the epoxy adhesive layer with a PE film, roll it into a roll, inspect and package it for storage, and store it in a frozen warehouse.
[0231] Before use, take the film out of the ice storage to restore to room temperature, cut the film into the required size, remove the PE film on the upper surface, press the film to the bonding surface by applying a certain pressure, then remove the silicone paper on the lower surface, overlap it with another adhesive and send it to the oven for curing. Stable bonding can be achieved by heating at 120℃ for 3 hours. After stable bonding, performance testing can be carried out.
[0232] Embodiment 4:
[0233] Prepare the epoxy film by the following steps:
[0234] 1) 30 g of bisphenol A liquid epoxy resin 128, 30 g of bisphenol A solid epoxy resin NPES-905L, 3 g of solid toughening agent Elvaloy PTW, and 10 g of toughening agent 3002 were weighed by mass fraction and added into a planetary mixer, the temperature was controlled at 130° C., and mixed for 2 h to obtain an intermediate;
[0235] 2) lowering the temperature to 80°C, adding 10g of latent curing agent dicyandiamide for 100s, 8g of curing accelerator DyhardUR500, 2g of BYK A530 and 2g of KH550 into a planetary mixer, controlling the temperature below 80°C, mixing for 45min, and obtaining a rubber compound;
[0236] 3) preheating the adhesive obtained in step 2) at a temperature of 60° C. for 30 min, and then hot-pressing the adhesive on silicone oil paper on an adhesive film making machine at a roller temperature of 80° C. to form a film, wherein the first surface of the epoxy adhesive layer is in contact with the silicone oil paper;
[0237] 4) Cover the second surface of the epoxy adhesive layer with a PE film, roll it into a roll, inspect and package it for storage, and store it in a frozen warehouse.
[0238] Before use, take the film out of the ice storage to restore to room temperature, cut the film into the required size, remove the PE film on the upper surface, press the film to the bonding surface by applying a certain pressure, then remove the silicone paper on the lower surface, overlap it with another adhesive and send it to the oven for curing. Stable bonding can be achieved by heating at 120℃ for 3 hours. After stable bonding, performance testing can be carried out.
[0239] Embodiment 5:
[0240] Prepare the epoxy film by the following steps:
[0241] 1) 40 g of bisphenol A liquid epoxy resin E44, 30 g of bisphenol A solid epoxy resin NPES-904, 3 g of MBS resin, and 12 g of toughening agent 3001 were weighed by mass fraction and added into a planetary mixer, the temperature was controlled at 130° C., and mixed for 2 h to obtain an intermediate;
[0242] 2) Lower the temperature to 80°C, continue to add 10g of latent curing agent dicyandiamide for 100s, 8g of curing accelerator DyhardUR300, 2g BYK A530 and 2g KH550 into a planetary mixer, control the temperature below 80°C, mix for 45min, and obtain a rubber compound;
[0243] 3) preheating the adhesive obtained in step 2) at a temperature of 60° C. for 30 min, and then hot-pressing the adhesive on silicone oil paper on an adhesive film making machine at a roller temperature of 80° C. to form a film, wherein the first surface of the epoxy adhesive layer is in contact with the silicone oil paper;
[0244] 4) Cover the second surface of the epoxy adhesive layer with a PE film, roll it into a roll, inspect and package it for storage, and store it in a frozen warehouse.
[0245] Before use, take the film out of the ice storage to restore to room temperature, cut the film into the required size, remove the PE film on the upper surface, press the film to the bonding surface by applying a certain pressure, then remove the silicone paper on the lower surface, overlap it with another adhesive and send it to the oven for curing. Stable bonding can be achieved by heating at 120℃ for 3 hours. After stable bonding, performance testing can be carried out.
[0246] Comparative Example 1: Example 1 was repeated, except that the latent curing agent Dyhard UR500 was not added.
[0247] Comparative Example 2: Example 1 was repeated, except that no MBS resin was added.
[0248] Comparative Example 3: Example 1 was repeated, except that 80 g of liquid epoxy resin bisphenol A type liquid epoxy resin NPEL-127E was added without adding solid epoxy resin.
[0249] Comparative Example 4: Example 1 was repeated, except that the liquid epoxy resin used was aromatic glycidyl ether type epoxy resin XY694.
[0250] Comparative Example 5: Example 1 was repeated, except that 2 g of ABS engineering plastic was used as the solid toughening agent.
[0251] The test results of the samples obtained in the above embodiments and comparative examples are shown in Table 1.
[0252] Table 1. Performance characterization data of samples prepared in Examples and Comparative Examples are as follows
[0253]
[0254] As can be seen from Table 1, the epoxy films added with solid toughening agents in Examples 1-5 have good peelability and can be cured at medium temperature. The epoxy films prepared in the present application have good bonding properties and have excellent bonding capabilities at room temperature, 100°C and -196°C.
[0255] The sample in Comparative Example 2 does not contain the solid toughening agent described in the first aspect of the present application. The sample in Comparative Example 3 does not contain a solid epoxy resin. The sample in Comparative Example 4 does not contain the liquid epoxy resin described in the first aspect of the present application, but contains an overactive aromatic glycidyl ether type epoxy resin XY694. Comparative Example 5 does not contain the solid toughening agent described in the first aspect of the present application, but contains ABS resin.
[0256] The results in Table 1 show that although the samples in Comparative Examples 2 to 5 can be completely cured, they cannot be peeled off from the release film, so they cannot be used normally in subsequent steps and their mechanical properties cannot be tested.
[0257] Comparison of the results of the comparative examples with those of the embodiments shows that in the epoxy adhesive of the present application, the use of a combination of a solid epoxy resin, a liquid epoxy resin, a solid toughening agent and a liquid toughening agent as described in the first aspect can prevent the adhesive from cross-linking during the process of forming into a film and the resulting adhesive film can be easily peeled off from the release film for subsequent use, and can also produce satisfactory bonding after the adhesive is cured at a temperature above 120°C, and such bonding provides excellent bonding strength over a wide temperature range (e.g., -196 to 100°C).
[0258] A person skilled in the art may make various changes to the present application according to the above description. Therefore, without violating the spirit of the claims of the present application, certain details in the embodiments shall not constitute a limitation on the present application, and the present application shall be protected within the scope defined by the attached claims.
Claims
1. An epoxy adhesive, comprising: a) a liquid epoxy resin, wherein the liquid epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, brominated bisphenol A epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, alicyclic epoxy resin, or a mixture thereof; preferably, the liquid epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, aliphatic glycidyl ether epoxy resin and glycidyl ester epoxy resin, or a mixture thereof; b) solid epoxy resin, preferably the solid epoxy resin is selected from: solid bisphenol A epoxy resin, solid bisphenol A novolac epoxy resin, bisphenol S glycidyl ether epoxy resin, glycidyl ester epoxy resin; more preferably, the solid epoxy resin is selected from isophthalic acid epoxy resin and trimesic acid epoxy resin; c) a solid toughening agent, wherein the solid toughening agent is selected from: styrene-butadiene rubber, MBS resin, ethylene-based terpolymer, or a mixture thereof; preferably, the melting point of the solid toughening agent is lower than 200° C., preferably lower than 190° C., preferably lower than 180° C., preferably lower than 170° C.; d) a latent curing agent, wherein the latent curing agent is selected from dicyandiamide, organic urea, modified amine, or a mixture thereof.
2. The epoxy adhesive of claim 1, wherein the liquid epoxy resin has an epoxide equivalent of 156 to 2500 g / eq, or 170 to 2200 g / eq, or 200 to 2000 g / eq, or 300 to 1800 g / eq, or 400 to 1700 g / eq, or 500 to 1600 g / eq, or 600 to 1500 g / eq, or 700 to 1200 g / eq, or 800 to 1100 g / eq, or 900 to 1000 g / eq; and / or The number average molar mass of the liquid epoxy resin is 300 to 500 g / mol; and / or The solid epoxy resin has an epoxy equivalent of 450 to 2500 g / eq, or 450 to 1700 g / eq, or 500 to 1600 g / eq, or 600 to 1500 g / eq, or 700 to 1200 g / eq, or 800 to 1100 g / eq, or 900 to 1000 g / eq; and / or; The number average molar mass of the solid epoxy resin is greater than 1000 g / mol.
3. The epoxy adhesive of claim 1, wherein the epoxy adhesive further comprises one or more of the following: e) Liquid toughening agent; Preferably, the liquid toughening agent is selected from: liquid nitrile rubber, liquid polysulfide rubber, polyether active toughening agent, rubber modified epoxy resin, polyurethane modified epoxy resin, or a combination thereof; Preferably, the liquid nitrile rubber is selected from HyPox 1300*8, HyPox 1300*13; Preferably, the rubber modified epoxy resin is selected from MX154, MX158; Preferably, the polyurethane modified epoxy resin is selected from SL3451 to SL3453; Preferably, the liquid toughening agent is selected from the liquid toughening agents with grades 3001, 3002, 801340, 901350 and RN55 purchased from Shanghai Huayi Resin Co., Ltd. f) curing accelerator; Preferably, the curing accelerator is selected from: imidazole and its derivatives, and amine adducts; more preferably, the curing accelerator is selected from DyhardUR500, DyhardUR300, PN-23, or MY-24; g) auxiliary agents; Preferably, the auxiliary agent is selected from: stabilizer, ultraviolet absorber, lubricant, pigment, dye, antistatic agent, nucleating agent, defoamer and coupling agent; preferably, the auxiliary agent is selected from defoamer and coupling agent; preferably, the coupling agent is a silane coupling agent.
4. The epoxy adhesive according to any one of claims 1 to 2, in: The content of the component a) liquid epoxy resin is 30 to 50 parts; and / or The content of the solid epoxy resin of component b) is 30 to 50 parts; and / or The content of the solid toughening agent of component c) is 0.1 to 5 parts; and / or The content of the latent curing agent of component d) is 5 to 15 parts; and / or The content of the component e) liquid toughening agent is 10 to 15 parts; and / or The content of the component f) curing accelerator is 1 to 10 parts; and / or The content of the auxiliary agent of component g) is 1 to 3 parts.
5. Epoxy film, including: - a layer of epoxy adhesive; and - a release film layer, wherein the epoxy adhesive comprises: a) a liquid epoxy resin, wherein the liquid epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, brominated bisphenol A epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, alicyclic epoxy resin, or a mixture thereof; preferably, the liquid epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, aliphatic glycidyl ether epoxy resin and glycidyl ester epoxy resin, or a mixture thereof; b) solid epoxy resin, preferably the solid epoxy resin is selected from: solid bisphenol A epoxy resin, solid bisphenol A novolac epoxy resin, bisphenol S glycidyl ether epoxy resin, glycidyl ester epoxy resin; more preferably, the solid epoxy resin is selected from isophthalic acid epoxy resin and trimesic acid epoxy resin; c) a solid toughening agent, wherein the solid toughening agent is selected from: styrene-butadiene rubber, MBS resin, ethylene-based terpolymer, or a mixture thereof; preferably, the melting point of the solid toughening agent is lower than 200° C., preferably lower than 190° C., preferably lower than 180° C., preferably lower than 170° C.; d) a latent curing agent, wherein the latent curing agent is selected from dicyandiamide, organic urea, modified amine, or a mixture thereof.
6. The epoxy film as claimed in claim 5, wherein the epoxy adhesive further comprises one or more of the following: e) Liquid toughening agent Preferably, the liquid toughening agent is selected from: liquid nitrile rubber, liquid polysulfide rubber, polyether active toughening agent, rubber modified epoxy resin, polyurethane modified epoxy resin, or a combination thereof; Preferably, the liquid nitrile rubber is selected from HyPox 1300*8, HyPox 1300*13; Preferably, the rubber modified epoxy resin is selected from MX154, MX158; Preferably, the polyurethane modified epoxy resin is selected from SL3451 to SL3453; Preferably, the liquid toughening agent is selected from the liquid toughening agents with grades 3001, 3002, 801340, 901350 and RN55 purchased from Shanghai Huayi Resin Co., Ltd.; f) curing accelerator; Preferably, the curing accelerator is selected from: imidazole and its derivatives, and amine adducts; more preferably, the curing accelerator can be selected from DyhardUR500, DyhardUR300, PN-23, or MY-24; g) Additives Preferably, the auxiliary agent is selected from: stabilizers, ultraviolet absorbers, lubricants, pigments, dyes, antistatic agents, nucleating agents, defoamers and coupling agents; preferably selected from defoamers and coupling agents; preferably, the coupling agent is a silane coupling agent.
7. The epoxy film according to any one of claims 5 to 6, wherein in the epoxy adhesive: The content of the component a) liquid epoxy resin is 30 to 50 parts; and / or The content of the solid epoxy resin of component b) is 30 to 50 parts; and / or The content of the solid toughening agent of component c) is 0.1 to 5 parts; and / or The content of the latent curing agent of component d) is 5 to 15 parts; and / or The content of the component e) liquid toughening agent is 10 to 15 parts; and / or The content of the component f) curing accelerator is 1 to 10 parts; and / or The content of the auxiliary agent of component g) is 1 to 3 parts.
8. A method for preparing the adhesive film according to any one of claims 5 to 6, the method comprising the following steps: 1) Mix the following components: a) a liquid epoxy resin, wherein the liquid epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, brominated bisphenol A epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, alicyclic epoxy resin, or a mixture thereof; preferably, the liquid epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, aliphatic glycidyl ether epoxy resin and glycidyl ester epoxy resin, or a mixture thereof; b) a solid epoxy resin, wherein the solid epoxy resin is in a solid state at room temperature; c) a solid toughening agent, wherein the solid toughening agent is selected from: styrene-butadiene rubber, MBS resin, ethylene-based terpolymer, or a mixture thereof; d) a latent curing agent, wherein the latent curing agent is selected from dicyandiamide, organic urea, modified amine, or a mixture thereof; 2) applying the mixture obtained in step 1) on a first release film to form an adhesive film, wherein the first surface of the epoxy adhesive layer is in contact with the first release film; 3) Optionally, a second release film layer is covered on the second surface of the epoxy adhesive layer.
9. A method for bonding different materials, the method comprising the following steps: 1) Applying an epoxy adhesive comprising: a) a liquid epoxy resin, wherein the liquid epoxy resin is selected from: bisphenol A epoxy resin, bisphenol F epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, or a mixture thereof; b) solid epoxy resin; c) a solid toughening agent, wherein the solid toughening agent is selected from: styrene-butadiene rubber, MBS resin, ethylene-based terpolymer, or a mixture thereof; d) a latent curing agent, wherein the latent curing agent is selected from dicyandiamide, organic urea, modified amine, or a mixture thereof; 2) contacting the second substrate with the surface of the first substrate with the adhesive to obtain a first laminate; 3) subjecting the first laminate to curing at a curing temperature greater than or equal to 120°C.
10. The method according to claim 9, in: In step 1), the mixed epoxy adhesive is directly applied to the first substrate, preferably by blade coating, spin coating, roller coating, drum coating, or drop coating; and / or Step 1) includes the following sub-steps: 1-1) preparing the adhesive film according to any one of claims 5 to 7 or the adhesive film prepared by the method according to claim 8; and 1-2) applying the adhesive layer in the adhesive film onto the first substrate so that the first surface of the adhesive layer is in contact with the first substrate.