High-wear-resistance friction material for electromagnetic brake and preparation method of high-wear-resistance friction material

By using high-temperature resistant resin and a variety of fiber reinforced materials in electromagnetic brakes, combining high specific heat capacity fillers and high-temperature friction reducers, the wear resistance and friction coefficient stability of friction materials is solved, extending the service life of electromagnetic brakes and reducing the use of electromagnetic brakes Maintenance frequency.

CN119019982APending Publication Date: 2024-11-26CHENGDU CHAODECHUANG TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411064405.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The friction materials used for existing electromagnetic brakes have poor wear resistance and poor friction coefficient stability, resulting in short service life and high maintenance frequency.

Method used

High temperature-resistant YSM resin powder is used as the adhesive, combined with carbon fiber, aramid pulp, basalt fiber, ceramic fiber, potassium titanate flakes and other reinforcement materials, and is equipped with feldspar powder, ice crystal powder, fluid silicon powder with high specific heat capacity and Fillers such as high-temperature friction reducing agents form friction materials with high wear resistance and high friction coefficient, and are prepared by hot pressing and sectioned heat treatment processes.

Benefits of technology

It significantly improves the high-temperature wear performance and friction coefficient stability of friction materials, extends the service life of electromagnetic brakes, and reduces the maintenance frequency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004978947220000091
    Figure BDA0004978947220000091
  • Figure BDA0004978947220000111
    Figure BDA0004978947220000111
Patent Text Reader

Abstract

The invention relates to the field of friction materials, and discloses a high-wear-resistance friction material for an electromagnetic brake and a preparation method of the high-wear-resistance friction material. The reinforcing material comprises carbon fibers, aramid pulp, basalt fibers, ceramic fibers, potassium titanate lamellar crystals and aluminum fibers; the filler comprises fluororubber powder, feldspar powder, high-temperature-resistant cashew nut shell oil friction powder, barite powder, crystalline flake graphite, granular graphite, a high-temperature antifriction agent, fluid silicon powder, cryolite powder, carbon black, zeolite powder, aluminum hydroxide, aluminum boride and an aluminum-magnesium-boron compound. According to the friction material provided by the invention, the proportions of the raw materials are utilized, so that the wear at different temperature stages can be reduced, the wear resistance of the friction material is improved, the high-low-temperature wear resistance of the friction material is improved, the high-temperature decline of the friction material is reduced, and the friction coefficient is stabilized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of friction materials, in particular to a high wear-resistant friction material for electromagnetic brakes and a preparation method thereof. Background Art

[0002] Electromagnetic brakes are mainly used in robots, aerial work vehicles, servo motors, lifting machinery and other industries. At present, most brakes achieve braking through friction between friction materials and counter-parts. Among them, due to the high frequency of use of lifting machinery, this requires that the core component of the electromagnetic brake, the friction material, must have very good wear resistance and a stable friction coefficient. At present, most friction materials use phenolic resin, rubber, etc. as adhesives, but phenolic resin and rubber have small molecular substances overflow when the temperature reaches 200°C, and the resin and rubber begin to decompose when the temperature exceeds 300°C. The operating temperature of electromagnetic brake friction materials is generally between 100 and 200°C, and the flash temperature of the contact surface may be as high as 800°C or more. When the adhesive begins to decompose, the friction material loses the bonding effect of the resin due to filler fibers and the wear rate increases. At present, the wear resistance of the friction material is generally improved by increasing the content of lubricating materials in the friction material, but to a certain extent, the friction coefficient of the friction material will be reduced, which will lead to a reduction in the torque of the electromagnetic brake.

[0003] Therefore, developing a friction material with high wear resistance and high friction coefficient for the lifting machinery industry has good market prospects. Summary of the invention

[0004] Technical problems solved by the present invention:

[0005] It is used to solve the problems of poor wear resistance of friction materials used in electromagnetic brakes of lifting machinery, poor stability of friction coefficient and short service life of electromagnetic brakes, extend the service life of lifting machinery brakes and reduce the maintenance frequency of electromagnetic brakes.

[0006] The technical solution adopted by the present invention is:

[0007] In view of the above technical problems, an object of the present invention is to provide a high wear-resistant friction material for electromagnetic brake and a preparation method thereof.

[0008] The specific contents are as follows:

[0009] First, the present invention provides a high wear-resistant friction material for electromagnetic brakes, wherein the raw material components include an adhesive, a reinforcing material, and a filler;

[0010] Reinforcement materials include carbon fiber, aramid pulp, basalt fiber, ceramic fiber, potassium titanate platelets, and aluminum fiber;

[0011] Fillers include fluororubber powder, feldspar powder, high temperature resistant cashew nut shell oil friction powder, barite powder, flake graphite, granular graphite, high temperature friction reducer, fluid silica powder, cryolite powder, carbon black, zeolite powder, aluminum hydroxide, aluminum boride, and aluminum magnesium boron compounds.

[0012] According to some preferred embodiments, the raw material components are measured by weight and include 12 to 16 parts of adhesive, 1 to 3 parts of carbon fiber, 1 to 3 parts of aramid pulp, 1 to 3 parts of basalt fiber, 5 to 8 parts of ceramic fiber, 5 to 10 parts of potassium titanate platelets, 2 to 5 parts of aluminum fiber, 5 to 8 parts of fluororubber powder, 6 to 10 parts of feldspar powder, 4 to 8 parts of high temperature resistant cashew nut shell oil friction powder, 10 to 15 parts of barite powder, 2 to 6 parts of flake graphite, 2 to 5 parts of granular graphite, 3 to 5 parts of high temperature friction reducer, 5 to 8 parts of fluid silicon powder, 3 to 5 parts of cryolite powder, 2 to 5 parts of carbon black, 2 to 6 parts of zeolite powder, 3 to 5 parts of aluminum hydroxide, 2 to 5 parts of aluminum boride, and 0.1 to 0.5 parts of aluminum magnesium boron compound.

[0013] In the above, the raw materials of the friction material are selected from the following components:

[0014] The first type: 13 parts of YSM resin powder, 1 part of carbon fiber, 2 parts of aramid pulp, 2 parts of basalt fiber, 6 parts of ceramic fiber, 5 parts of potassium titanate platelets, 3 parts of aluminum fiber, 5 parts of fluororubber powder, 6 parts of feldspar powder, 5 parts of high temperature cashew nut shell oil friction powder, 12 parts of barite powder, 3 parts of flake graphite, 4 parts of granular graphite, 5 parts of high temperature friction reducer, 8 parts of fluid silicon powder, 5 parts of cryolite powder, 2 parts of carbon black, 6 parts of zeolite powder, 3 parts of aluminum hydroxide, 5 parts of aluminum boride, and 0.3 parts of aluminum magnesium boron compound;

[0015] The second type: 15 parts of YSM resin powder, 2 parts of carbon fiber, 2 parts of aramid pulp, 1 part of basalt fiber, 8 parts of ceramic fiber, 6 parts of potassium titanate platelets, 4 parts of aluminum fiber, 8 parts of fluororubber powder, 8 parts of feldspar powder, 4 parts of high temperature cashew nut shell oil friction powder, 10 parts of barite powder, 4 parts of flake graphite, 5 parts of granular graphite, 4 parts of high temperature friction reducer, 6 parts of fluid silicon powder, 4 parts of cryolite powder, 3 parts of carbon black, 4 parts of zeolite powder, 5 parts of aluminum hydroxide, 4 parts of aluminum boride, and 0.2 parts of aluminum magnesium boron compound;

[0016] The third type: 14 parts of YSM resin powder, 3 parts of carbon fiber, 1 part of aramid pulp, 3 parts of basalt fiber, 5 parts of ceramic fiber, 8 parts of potassium titanate platelets, 5 parts of aluminum fiber, 6 parts of fluororubber powder, 10 parts of feldspar powder, 6 parts of high temperature resistant cashew nut shell oil friction powder, 13 parts of barite powder, 2 parts of flake graphite, 4 parts of granular graphite, 3 parts of high temperature friction reducer, 5 parts of fluid silica powder, 3 parts of cryolite powder, 5 parts of carbon black, 5 parts of zeolite powder, 4 parts of aluminum hydroxide, 4 parts of aluminum boride, and 0.1 parts of aluminum magnesium boron compound.

[0017] The following description is made about the raw material components of the friction material mentioned above:

[0018] 1. Adhesive

[0019] Using high temperature resistant YSM resin powder as adhesive can significantly increase the decomposition temperature of the friction material matrix and improve the high temperature wear resistance of the friction material.

[0020] 2. Reinforcement Materials

[0021] Carbon fiber powder, aramid pulp, modified basalt fiber, ceramic fiber, potassium titanate platelets, and aluminum fiber are used as reinforcing materials. The synergistic reinforcement effect of multiple fibers is used to improve the strength and thermal decomposition temperature of the resin matrix. The aluminum fiber is made by scraping a round rod. The fiber is rough on all four sides, uniform in thickness, and has many curls. Therefore, the aluminum fibers can be linked to each other to form a body network. Due to the rough surface of the aluminum fiber, it can grab more organic fibers and inorganic fibers, so that the fibers form a tree-like structure, which can effectively improve the strength of the friction material matrix. At the same time, the heat on the friction surface can also be dissipated through the network structure formed by the aluminum fiber, thereby reducing the temperature of the friction surface. Aluminum is soft and has large plastic deformation. It has a certain lubrication and friction reduction effect during the friction process. Potassium titanate has low thermal conductivity and a negative temperature coefficient, that is, the higher the temperature, the lower the thermal conductivity. Therefore, potassium titanate can isolate part of the friction heat on the surface at high temperature and slow down the thermal decomposition of the resin. At the same time, potassium titanate platelets can promote the breakage of the phenolic resin molecular chain, which is beneficial to the formation and stability of the transfer film on the friction surface.

[0022] Modified basalt fiber is obtained by removing impurities from basalt, putting it into a modification solution, and then treating it with a silane coupling agent; impurity removal treatment: vacuum heat treatment at 500-600℃ for 0.5-2h; modification solution: V 双氧水 :V 饱和氨水 :V 饱和氢氧化钙 =1:1:1. Modification treatment: soak at 40-70℃ for 18-36h; silane coupling agent is KH-550, and the silane coupling agent is configured into a solution, V 硅烷偶联剂 :V 水 :V 乙醇 =5~15:60~80:10~30. The modified basalt fiber is used to make its surface rougher and have stronger grip on the material. After being modified with alkali solution, the defects and holes on the fiber surface will be eroded, the remaining fiber surface will become rough, and the fiber strength will also be enhanced. A large number of active groups will be generated on the surface of the basalt fiber modified by silane coupling agent, which greatly enhances the bonding performance of the resin, improves the bonding strength, and then improves the high temperature resistance of the resin matrix.

[0023] 3. Filling

[0024] Feldspar powder: Feldspar powder is a high specific heat capacity filler, which can produce phase change and heat absorption of cryolite powder at different temperatures. The specific heat capacity of feldspar powder is 1.32J / (g·℃), while the specific heat capacity of commonly used inorganic mineral fillers is usually less than 0.7J / (g·℃). Under the same conditions, feldspar powder can absorb more heat than other fillers, while cryolite has obvious phase change or melting endothermic reaction at 570℃, 730℃ and 930℃, which has a significant effect on improving the high temperature stability of friction materials. The synergistic effect of feldspar powder and cryolite powder can greatly reduce the heat transfer of friction materials.

[0025] Fluid silicon powder: Fluid silicon powder is a new covalent crystal - zirconium silicide, which is formed by gasifying silicon powder and an appropriate amount of zirconium element through electric melting heating. It is a ceramic material with high hardness, high melting point, high electrical conductivity, high thermal conductivity, and good high temperature thermal shock resistance; it can significantly improve the high and low temperature friction coefficient of friction materials. Compared with other silicon micropowders, fluid silicon powder has low oxide content, high purity, small average particle size, and high thermal conductivity. Combined with resin and rubber, it can improve the strength, toughness, wear resistance and high temperature resistance of friction materials, while increasing its aging resistance, and plays a good reinforcing role in friction materials. Fluid silicon powder can greatly improve the stability of the friction coefficient of friction materials and reduce thermal decay.

[0026] High-temperature friction reducer: High-temperature friction reducer is used to improve the wear resistance in the high-temperature stage. To expand, that is to say: the high-temperature friction reducer is obtained by adding metal oxides and metal sulfides to the quick-dissolving sodium silicate as the base material. The metal oxide includes at least one of aluminum oxide, zirconium oxide, and zinc oxide; the metal sulfide includes at least one of zinc sulfide, tin sulfide, and ferrous sulfide. The components of the high-temperature friction reducer are calculated by mass: 10-20 parts of quick-dissolving sodium silicate, 1-3 parts of aluminum oxide, 1-3 parts of zirconium oxide, 1-3 parts of zinc oxide, 3-5 parts of zinc sulfide, and 2-5 parts of tin sulfide. Preferably, 15 parts of quick-dissolving sodium silicate, 2 parts of aluminum oxide, 2 parts of zirconium oxide, 2 parts of zinc oxide, 3 parts of zinc sulfide, and 5 parts of tin sulfide. Add the above components to the ball mill for ball milling and mixing, the ball mill speed is 1000r / min, and the ball milling time is 30min. After ball milling, it is dried at 80°C, and after drying for 60 minutes, it is sieved to obtain a high-temperature friction reducer. Instant sodium silicate is mixed with alumina and zinc oxide to obtain a material with high porosity and high specific surface area, which can improve the high-temperature bonding strength. During the pressing process, when the temperature reaches 100°C, the instant sodium silicate is partially dehydrated during the pressing process, and forms a gel-like substance with alumina and zinc oxide, which improves the bonding strength. When the temperature reaches 180-200°C, aluminum hydroxide continues to decompose, releases water molecules, and continues to react to generate gelling substances, further improving the bonding strength. When the temperature reaches 400°C, tin sulfide decomposes, isolates oxygen, and delays the decomposition of the resin. When the temperature reaches 650°C, zinc sulfide decomposes and delays the decomposition of the resin. When the temperature reaches 880°C, tin sulfide melts and plays a certain bonding role. High-temperature friction reducers can enhance adhesion at different temperature stages and reduce the reduction in bonding strength caused by resin decomposition. The material has good bonding with resin and can play a good reinforcing role. When the resin decomposes at high temperature, it can be used as a high-temperature lubricant and inorganic binder to reduce wear and stabilize the friction coefficient. During the friction braking process, the high-temperature friction reducer attaches a protective film on the friction surface to reduce the oxidation and decomposition of organic matter such as resin and air (oxygen), thereby increasing the service life of the product. It is a new type of green and environmentally friendly material. During use, it can inhibit the combustion of organic matter such as resin and rubber, prevent the generation of undesirable conditions such as smoke and odor, and does not produce toxic gases. It can greatly improve the temperature resistance of friction materials. The high-temperature friction reducer can synergize with flake graphite, granular graphite, and aluminum-magnesium-boron compounds. The coarse and fine combination of granular graphite can reduce the direct gasification of fine graphite at high temperature, which leads to a decrease in the lubrication effect of graphite. The high-temperature friction reducer can lubricate and reduce friction at high temperature stages, and synergistically reduce high and low temperature wear. At the same time, granular graphite has fine pores that can absorb the gas generated by high-temperature carbonization, reduce the generation of air cushion film, reduce thermal decay, and improve the stability of high-temperature friction coefficient.

[0027] Aluminum hydroxide is an amphoteric hydroxide with a Mohs hardness of 3. It is often used as a friction-increasing filler and also as a flame retardant material. Aluminum hydroxide dehydrates and absorbs heat in the range of 180-200°C to generate aluminum oxide and water vapor. The aluminum oxide generated on the friction surface can isolate part of the heat from propagating inward, and the generated water vapor can take away a large amount of heat, which has a good cooling effect. Since the generated water vapor will cause the friction coefficient to decrease, the zeolite powder can absorb part of the water vapor, and part of the water vapor will react with the fast-dissolving sodium silicate. Zeolite is a framework-like hydrated alkali or alkaline earth metal aluminosilicate mineral. Its crystal water exists as a water molecule, which is different from the general structural water (-OH). Therefore, when heated at a certain temperature, the lattice is not destroyed after dehydration, and there are still gaps in the position of the original water molecules, forming a sponge lattice structure, which has the characteristic of re-absorbing water vapor and other gases into the gaps. When the temperature rises, the zeolite gaps become larger and allow molecules to enter. When cooling, the molecules that enter are trapped in the gaps and retained for a long time until they are heated again and released. Therefore, the synergistic effect of aluminum hydroxide and zeolite powder can be used to reduce the friction surface temperature and delay the decomposition of resin by utilizing the heat absorption of aluminum hydroxide decomposition. The decomposed aluminum oxide can stabilize the high-temperature friction coefficient, while water vapor is absorbed by zeolite powder and instant sodium silicate, reducing the influence of water vapor on the friction coefficient.

[0028] Fluororubber: Fluororubber has excellent wear resistance, high temperature resistance, corrosion resistance, etc. Adding it to friction materials can improve the durability and wear resistance of brake materials, while reducing noise and vibration. Carbon black is a black pigment with good thermal stability and strong UV resistance. It is widely used in rubber, plastic and other materials to improve the mechanical strength, heat resistance, weather resistance, etc. of the materials. The synergistic effect of carbon black and fluororubber can improve the wear resistance and toughness of fluororubber, and indirectly improve the wear resistance and toughness of friction materials. Similarly, carbon black can also be added to resin materials to increase their strength and wear resistance.

[0029] High temperature resistant cashew nut shell oil friction powder (black powder): Its thermal decomposition temperature is as high as 300℃, which has the function of stabilizing the high and low temperature friction coefficient and has a significant effect in reducing high and low temperature wear. Barite can be used as a space filler to reduce costs. It can stabilize the friction coefficient and form a stable friction interface layer at high temperature. It only has a polishing effect on the mating parts and has little wear.

[0030] Aluminum boride: It is a metal ceramic material synthesized from aluminum and boron. Aluminum borides include AlB2, AlB4 and AlB 12, contains two chemical bonds, metallic bonds and covalent bonds, and has excellent performance at high temperatures. The characteristics of covalent bonds are high hardness and high melting point, and its melting point is about 2200℃. Because aluminum boride contains metallic bonds, it has a high thermal conductivity of about 200W / (m·K), which is much higher than most metal materials and has excellent thermal conductivity. Adding aluminum boride to friction materials can improve the high-temperature strength and high-temperature wear resistance of friction materials, and at the same time can accelerate the heat diffusion of the friction surface, reduce the temperature rise of the friction surface, delay the decomposition of the resin, and improve the high-temperature wear resistance of the friction material.

[0031] Aluminum magnesium boron compound (AlMgB 14 )(BAM): Its hardness is second only to diamond and boron nitride, and it has a very low friction coefficient and good high temperature resistance. The hardness of boron, magnesium and aluminum alloys is as high as 32GPa. Adding friction materials can improve the high temperature strength of friction materials. Its friction coefficient with steel is as low as 0.02, while the friction coefficient of polytetrafluoroethylene is 0.04-0.1. It has excellent lubrication and friction reduction effects and can be used as a lubrication and friction reduction material under extreme working conditions. Therefore, adding it to the friction material can greatly reduce its wear, especially wear under extreme working conditions. Adding a small amount of aluminum-magnesium-boron compounds, synergistically with graphite and high-temperature friction reducers, reduces wear at different temperature stages, greatly delays the high-temperature decomposition of resin, and improves the wear resistance of friction materials.

[0032] Second, the present invention provides a method for preparing the aforementioned high wear-resistant friction material for electromagnetic brake, comprising the following steps:

[0033] S1 Mixing

[0034] Carbon fiber powder, aramid pulp and basalt fiber are blended to obtain blend A; ceramic fiber, potassium titanate platelets, aluminum fiber, fluororubber powder, feldspar powder, high temperature resistant cashew nut shell oil friction powder, barite powder, flake graphite, granular graphite, high temperature friction reducer, cryolite powder, carbon black, zeolite powder, aluminum hydroxide, aluminum boride and aluminum magnesium boron compound are added to blend A to obtain blend B;

[0035] S2 Hot Press

[0036] The blend B is subjected to hot pressing to obtain a semi-finished product;

[0037] S3 Heat Treatment

[0038] The semi-finished product is heated in stages to obtain the finished product.

[0039] According to some preferred embodiments, in S2, the pressing temperature is 150-160°C, the pressing pressure is 30-40 MPa, and the pressure holding is performed at 60-80 s / mm.

[0040] According to some preferred embodiments, in S3, the staged heating includes stage I, stage II, stage III, and stage IV;

[0041] Stage I: from room temperature to 135-145°C, heating for 1 hour, keeping warm for 1-2 hours;

[0042] Stage II: from 135-145℃ to 155-165℃, heating for 30min, keeping warm for 2-3h;

[0043] Stage III: from 155-165℃ to 185-195℃, heating for 30min, keeping warm for 1-2h;

[0044] Stage IV: Increase the temperature from 185-195°C to 205-215°C, increase the temperature for 30 minutes, and keep warm for 2-3 hours.

[0045] The beneficial effects achieved by the present invention are:

[0046] The present invention improves the high-temperature wear performance of the friction material by selecting high-temperature resistant resin, fiber-reinforced material and high specific heat and heat-absorbing filler, and adopts special high-temperature friction reducer, flake graphite and granular graphite for use in combination to reduce wear at different temperature stages and improve the wear resistance of the friction material. On the friction surface, potassium titanate flakes and aluminum oxide formed by the decomposition of aluminum hydroxide can isolate part of the heat, and the decomposition of aluminum hydroxide, the heat absorption of feldspar powder and the phase change of cryolite further reduce the heat transmission. The remaining heat is quickly conducted away through aluminum fiber and aluminum boride, which reduces the contact surface temperature and delays the decomposition of the resin. The flake graphite, granular graphite, high-temperature friction reducer and aluminum-magnesium-boron compound are used for lubrication, which greatly improves the high and low temperature wear resistance of the friction material. The porous granular graphite and zeolite powder can adsorb small molecular substances, reduce the high-temperature decay of the friction material, and stabilize the friction coefficient. DETAILED DESCRIPTION

[0047] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0048] Examples 1-3, Comparative Examples 1-3

[0049] Each embodiment provided by the present invention uses a high temperature resistant adhesive, reinforcing fiber and filler to prepare a friction material for a lifting machinery electromagnetic brake. The ratio of the friction material is calculated by mass fraction. The comparative example and the embodiment use the same production process, production equipment, process parameters, and product size. The specific ratio is shown in Table 1.

[0050] Table 1 Friction material formulation (Example-E, Comparative Example-C)

[0051]

[0052] in:

[0053] The preparation method of modified basalt fiber is as follows: calcining basalt fiber in vacuum at 500-600℃ for 1h to remove impurities such as organic matter on the surface. Soaking the calcined basalt fiber in a modified solution for 24h at a temperature of 50℃. The modified solution is a mixture of hydrogen peroxide, saturated ammonia water, and saturated calcium hydroxide solution in a volume ratio of 1:1:1. After soaking, rinse the basalt fiber with distilled water. Then, soak the rinsed basalt fiber in KH550 solution (the volume ratio of KH550 solution is water: ethanol: silane = 10:70:20) for 24h, take it out and dry it at 120℃ for 1h.

[0054] The preparation method of the high-temperature friction reducer is as follows: weigh 15 parts of instant sodium silicate, 2 parts of aluminum oxide, 2 parts of zirconium oxide, 2 parts of zinc oxide, 3 parts of zinc sulfide, and 5 parts of tin sulfide. Add the above components into a ball mill for ball milling and mixing, the ball mill speed is 1000r / min, and the ball milling time is 30min. After ball milling, dry at 80°C, dry for 60min, and then sieve to obtain the high-temperature friction reducer.

[0055] The preparation method of the friction material of the lifting machinery electromagnetic brake provided above is:

[0056] (1) Mixing: Weigh the raw materials of each component according to the proportion, mix the carbon fiber powder, aramid pulp and basalt fiber in a plowshare mixer for 3 to 5 minutes to evenly disperse the carbon fiber powder, aramid pulp and modified basalt fiber to obtain blend A, and add the remaining other components into the plowshare mixer and mix for 15 to 20 minutes to obtain blend B. The main shaft speed of the mixer is 200 to 300 r / min, and the reamer speed is 1000 to 2000 r / min.

[0057] (2) Hot pressing: Use a 100T four-column hydraulic press to evenly spread blend B into the mold and press it. The pressing temperature is 150-160°C, the pressing pressure is 30-40MPa, and the pressure is maintained for 60-80s / mm. Exhaust gas is performed before pressure maintenance. Press for 10s and exhaust gas for 5s. After 3-5 exhaust gas cycles, the pressure maintenance stage begins. After the pressure maintenance stage, the semi-finished friction material is obtained.

[0058] (3) Heat treatment: heat from room temperature to 140°C over 1 h, keep warm for 1-2 h, heat from 140°C to 160°C over 30 min, keep warm for 2-3 h, heat from 160°C to 190°C over 30 min, keep warm for 1-2 h, heat from 190°C to 210°C over 30 min, keep warm for 6-8 h, then cool to 50°C and take out.

[0059] The friction materials prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were used as samples and tested according to the relevant requirements of GB / T11834 friction plates for industrial and agricultural machinery. The test results are shown in Table 2.

[0060] Table 2 Friction material constant speed test results (Example-E, Comparative Example-C)

[0061]

[0062] The friction material is made into a finished brake product with the specification of Z627-Z12ZT (180V) 42H22.5-P, requiring a torque greater than 42N·m and a clearance of 0.25 to 0.35mm. The test is carried out in accordance with the relevant requirements of GB / T 34114-2017 "General Technical Requirements for Electromagnetic Brakes for Motors". The motor and brake are started and stopped at the same time, with a speed of 3000rpm and a moment of inertia of 0.00472kg*m 2 , run for 6s and stop for 4s, emergency braking times 320 times / h, test time 1h. The test results are shown in Table 3.

[0063] Table 3 Friction material emergency brake test results (Example-E, Comparative Example-C)

[0064] Measurement conditions E1 E2 E3 C1 C2 C3 Torque before test 48 43 46 46 44 49 Torque after test 85 79 86 90 82 95 Pre-test clearance 0.33 0.28 0.3 0.29 0.27 0.31 Post-test clearance 0.33 0.29 0.31 0.32 0.31 0.35

[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A high wear-resistant friction material for electromagnetic brake, characterized in that: The raw material components include adhesives, reinforcing materials, and fillers; Reinforcement materials include carbon fiber, aramid pulp, basalt fiber, ceramic fiber, potassium titanate platelets, and aluminum fiber; Fillers include fluororubber powder, feldspar powder, high temperature resistant cashew nut shell oil friction powder, barite powder, flake graphite, granular graphite, high temperature friction reducer, fluid silica powder, cryolite powder, carbon black, zeolite powder, aluminum hydroxide, aluminum boride, and aluminum magnesium boron compounds.

2. The high wear-resistant friction material for electromagnetic brake according to claim 1, characterized in that: The raw material components are calculated by weight and include 12-16 parts of adhesive, 1-3 parts of carbon fiber, 1-3 parts of aramid pulp, 1-3 parts of basalt fiber, 5-8 parts of ceramic fiber, 5-10 parts of potassium titanate platelets, 2-5 parts of aluminum fiber, 5-8 parts of fluororubber powder, 6-10 parts of feldspar powder, 4-8 parts of high-temperature resistant cashew nut shell oil friction powder, 10-15 parts of barite powder, 2-6 parts of flake graphite, 2-5 parts of granular graphite, 3-5 parts of high-temperature friction reducer, 5-8 parts of fluid silicon powder, 3-5 parts of cryolite powder, 2-5 parts of carbon black, 2-6 parts of zeolite powder, 3-5 parts of aluminum hydroxide, 2-5 parts of aluminum boride, and 0.1-0.5 parts of aluminum magnesium boron compound.

3. The high wear-resistant friction material for electromagnetic brake according to claim 2, characterized in that: The raw materials of the friction material can be selected from the following components: The first type: 13 parts of YSM resin powder, 1 part of carbon fiber, 2 parts of aramid pulp, 2 parts of basalt fiber, 6 parts of ceramic fiber, 5 parts of potassium titanate platelets, 3 parts of aluminum fiber, 5 parts of fluororubber powder, 6 parts of feldspar powder, 5 parts of high temperature cashew nut shell oil friction powder, 12 parts of barite powder, 3 parts of flake graphite, 4 parts of granular graphite, 5 parts of high temperature friction reducer, 8 parts of fluid silicon powder, 5 parts of cryolite powder, 2 parts of carbon black, 6 parts of zeolite powder, 3 parts of aluminum hydroxide, 5 parts of aluminum boride, and 0.3 parts of aluminum magnesium boron compound; The second type: 15 parts of YSM resin powder, 2 parts of carbon fiber, 2 parts of aramid pulp, 1 part of basalt fiber, 8 parts of ceramic fiber, 6 parts of potassium titanate platelets, 4 parts of aluminum fiber, 8 parts of fluororubber powder, 8 parts of feldspar powder, 4 parts of high temperature cashew nut shell oil friction powder, 10 parts of barite powder, 4 parts of flake graphite, 5 parts of granular graphite, 4 parts of high temperature friction reducer, 6 parts of fluid silicon powder, 4 parts of cryolite powder, 3 parts of carbon black, 4 parts of zeolite powder, 5 parts of aluminum hydroxide, 4 parts of aluminum boride, and 0.2 parts of aluminum magnesium boron compound; The third type: 14 parts of YSM resin powder, 3 parts of carbon fiber, 1 part of aramid pulp, 3 parts of basalt fiber, 5 parts of ceramic fiber, 8 parts of potassium titanate platelets, 5 parts of aluminum fiber, 6 parts of fluororubber powder, 10 parts of feldspar powder, 6 parts of high temperature resistant cashew nut shell oil friction powder, 13 parts of barite powder, 2 parts of flake graphite, 4 parts of granular graphite, 3 parts of high temperature friction reducer, 5 parts of fluid silica powder, 3 parts of cryolite powder, 5 parts of carbon black, 5 parts of zeolite powder, 4 parts of aluminum hydroxide, 4 parts of aluminum boride, and 0.1 parts of aluminum magnesium boron compound.

4. The high wear-resistant friction material for electromagnetic brake according to any one of claims 1 to 3, characterized in that: Each raw material of the friction material includes at least one of the characteristics (1) to (3): (1) The adhesive is YSM resin powder; (2) Basalt fiber is modified: after the basalt is impurity-free, it is put into a modification solution and then treated with a silane coupling agent to obtain modified basalt fiber; (3) High temperature friction reducer is made of quick-dissolving sodium silicate as base material, with metal oxides and metal sulfides added.

5. The high wear-resistant friction material for electromagnetic brake according to claim 4, characterized in that: Feature (2) includes at least one of features (2-1) to (2-4): (2-1) Impurity removal treatment: vacuum heat treatment at 500-600°C for 0.5-2h; (2-2) Modified solution: V 双氧水 :V 饱和氨水 :V 饱和氢氧化钙 =1:1:1; (2-3) Modification treatment: soak at 40-70°C for 18-36h; (2-4) The silane coupling agent is KH-550, and the silane coupling agent is prepared into a solution, V 硅烷偶联剂 :V 水 :V 乙醇 =5~15:60~80:10~30.

6. The high wear-resistant friction material for electromagnetic brake according to claim 4, characterized in that: Feature (3) includes at least one of features (3-1) to (3-3): (3-1) The metal oxide includes at least one of aluminum oxide, zirconium oxide and zinc oxide; (3-2) The metal sulfide includes at least one of zinc sulfide, tin sulfide and ferrous sulfide; (3-3) The mass ratio of quick-dissolving sodium silicate, metal oxide and metal sulfide is 10-20:3-9:3-12.

7. The high wear-resistant friction material for electromagnetic brake according to claim 6, characterized in that: Feature (3-3) includes feature (3-3-1): (3-3-1) The mass ratio of quick-dissolving sodium silicate, aluminum oxide, zirconium oxide, zinc oxide, zinc sulfide and tin sulfide is 10-20:1-3:1-3:1-3:3-5:2-5.

8. The method for preparing a high wear-resistant friction material for an electromagnetic brake according to any one of claims 1 to 7, characterized in that: The steps include: S1 Mixing Carbon fiber powder, aramid pulp and basalt fiber are blended to obtain blend A; ceramic fiber, potassium titanate platelets, aluminum fiber, fluororubber powder, feldspar powder, high temperature resistant cashew nut shell oil friction powder, barite powder, flake graphite, granular graphite, high temperature friction reducer, fluid silicon powder, cryolite powder, carbon black, zeolite powder, aluminum hydroxide, aluminum boride and aluminum magnesium boron compound are added to blend A to obtain blend B; S2 Hot Press The blend B is subjected to hot pressing to obtain a semi-finished product; S3 Heat Treatment The semi-finished product is heated in stages to obtain the finished product.

9. The method for preparing a high wear-resistant friction material for an electromagnetic brake according to claim 8, characterized in that: In S2, the pressing temperature is 150-160°C, the pressing pressure is 30-40 MPa, and the pressure holding is performed at 60-80 s / mm.

10. The method for preparing a high wear-resistant friction material for an electromagnetic brake according to claim 8, characterized in that: In S3, the staged heating includes stage I, stage II, stage III, and stage IV; Stage I: from room temperature to 135-145°C, heating for 1 hour, keeping warm for 1-2 hours; Stage II: from 135-145℃ to 155-165℃, heating for 30min, keeping warm for 2-3h; Stage III: from 155-165℃ to 185-195℃, heating for 30min, keeping warm for 1-2h; Stage IV: Increase the temperature from 185-195°C to 205-215°C, increase the temperature for 30 minutes, and keep warm for 2-3 hours.

Citation Information

Cited By

  • Aramid pulp with bionic plant branch fractal structure and preparation process thereof

    CN119980750A