Energy storage medium and preparation method and application thereof
The high-efficiency energy storage medium encapsulated by the organic-inorganic hybrid method and the alginic acid microcapsule method solves the problems of treatment agent failure and tool failure caused by the increase in the drilling fluid temperature, achieves rapid cooling and improves the cooling efficiency of the drilling fluid.
Patent Information
- Application Number
- CN202310594971.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
AI Technical Summary
During the oil and natural gas development process, the increase in the drilling fluid temperature leads to the failure of the treatment agent and the failure of the downhole tool. The existing cooling methods consume high energy and have poor heat dissipation effects, making it difficult to quickly cool down.
The organic-inorganic hybridization method is used to form composite energy storage materials and are encapsulated by alginic acid microcapsule method to form a high-efficiency energy storage medium to quickly reduce the drilling fluid temperature.
The heat absorption efficiency is improved, rapid cooling is achieved, and the cooling effect of drilling fluid temperature is significantly improved. The cooling efficiency is greater than that of conventional water and air cooling.
Smart Images

Figure BDA0004246820630000141 
Figure BDA0004246820630000151
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of drilling fluid, and in particular relates to an energy storage medium and a preparation method and application thereof. Background Art
[0002] At present, in the process of oil and gas development, the formations being drilled are getting deeper and deeper, and the formation temperatures are getting higher and higher, which will bring more negative effects. One of them is that the performance of the drilling fluid will deteriorate. Most of the treatment agents in the drilling fluid have a certain temperature resistance. When the temperature rises to a certain level, chain breaking or disproportionation reactions will occur, resulting in the failure of the treatment agent. More seriously, when the temperature rises to above 200°C, the most commonly used montmorillonite in the drilling fluid will dehydrate; the second negative effect is that most downhole tools will cause internal components to fail under high temperature conditions, resulting in tool failure, and the drill has to be frequently pulled up and down to replace the drill bit, which will reduce the effective drilling operation time. More seriously, if the operation time in a certain layer is too long, it may sometimes cause serious problems such as stuck drill or instability of the well wall, which will bring serious losses. For this reason, it is necessary to adopt an effective method to reduce the temperature of the drilling fluid. The current method to reduce the temperature of the drilling fluid is the natural reduction method, or the water cooling system is introduced into the ground circulation system of the drilling fluid, but this method consumes a lot of energy and has poor heat dissipation effect.
[0003] At present, there is a method of storing energy by adding paraffin particles underground and cooling the well by dissipating heat on the ground. This method has a certain effect, but the amount of paraffin required is very high and it will also have a certain impact on the performance of the drilling fluid. At the same time, these paraffins will inevitably cause certain losses during the circulation process. Therefore, it is more realistic to find a more effective energy storage fluid in the ground cooling circulation system.
[0004] Invention patent 200510038602.7 proposes a method for making microcapsules of phase change energy storage materials, using tetradecane or pentadecane as organic phase change materials, and using a mixture of natural linalool and gum arabic to make an outer capsule to form a phase change material, and its phase change temperature is 5-12°C. Tetradecane or pentadecane is easy to deform at high temperatures and absorbs relatively low heat.
[0005] Invention patent 201611184478.X discloses a composite phase change material and its preparation method. It includes an organic phase change material and an inorganic carrier, the organic phase change material fills the pores of the inorganic carrier, the organic phase change material is polyethylene glycol, the inorganic carrier is expanded graphite, and the mass ratio of polyethylene glycol to the expanded graphite is 11.5:1. It belongs to a solid phase change material, not a phase change fluid. Summary of the invention
[0006] The purpose of the present invention is to meet the demand for rapid cooling of the drilling fluid temperature at the well site outlet that is too high, and to solve the defects of the currently commonly used water cooling technology that has less energy storage and is difficult to cool quickly. The present invention mainly adopts an organic-inorganic hybrid method to form a composite energy storage material, and encapsulates it through an alginate microcapsule method to form a high-efficiency energy storage material. The high-concentration energy storage material can be used to quickly reduce the drilling fluid temperature through density circulation.
[0007] In a first aspect, the present invention proposes an energy storage medium, which comprises, by mass percentage, 50% to 70% deionized water, 0.2% to 5.0% viscosity enhancer, and 40% to 50% organic-inorganic hybrid core material / alginate microspheres.
[0008] As a specific embodiment of the present invention, the viscosity enhancer includes one or any combination of polyacrylamide, hydroxymethyl cellulose, and carboxymethyl starch, and the number average molecular weight of the viscosity enhancer is 500×10 4 ~1000×10 4 .
[0009] As a specific embodiment of the present invention, the diameter of the organic-inorganic hybrid core material / alginate microspheres is 1 mm to 5 mm, the wall thickness is 0.1 mm to 0.5 mm, and the mass percentage of the organic-inorganic hybrid core material to the microspheres is 80% to 92%.
[0010] As a specific embodiment of the present invention, the preparation method of the organic-inorganic hybrid core material / alginate microspheres includes: reacting and curing the organic-inorganic hybrid core material and sodium alginate under the action of a curing agent.
[0011] As a specific embodiment of the present invention, the reaction conditions include: temperature of 70°C to 90°C, stirring speed of 1000rpm to 3000rpm, and reaction time of 30min to 60min; the curing conditions include: stirring speed of 100rpm to 500rpm, and curing time of 12h to 24h;
[0012] As a specific embodiment of the present invention, the curing agent is one of calcium chloride, calcium bromide, and calcium nitrate, or a combination of any two thereof.
[0013] Exemplarily, the method for preparing organic-inorganic hybrid core material / alginate microspheres comprises the following steps:
[0014] 1) In a closed autoclave, add 800g-1500g of organic-inorganic hybrid core material, 1600g-2000g of sodium alginate and 3000g-3500g of deionized water, raise the system temperature to 70°C-90°C, adjust the stirring speed to 1000rpm-3000rpm, and stir and disperse for 30min-60min;
[0015] 2) Add 400g to 800g of curing agent to the above reactor, reduce the stirring speed to 100rpm to 500rpm, and solidify into balls for 12h to 24h;
[0016] 3) After the reaction is completed, the generated microspheres are fished out and washed three times with deionized water, and the millimeter-sized microspheres are screened out by centrifugal screening;
[0017] 4) The system is then transferred to a rotary evaporator to remove the remaining solvent, and the obtained microspheres are organic-inorganic hybrid core material / alginate microspheres.
[0018] As a specific embodiment of the present invention, the raw materials for preparing the organic-inorganic hybrid core material include polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer, nano nucleating agent, alkali provider and sodium montmorillonite.
[0019] As a specific embodiment of the present invention, the preparation of the organic-inorganic hybrid core material includes the following steps:
[0020] 1) adding a nano nucleating agent to the dissolved polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer to react to obtain a first reaction product;
[0021] 2) adding deionized water and an alkali provider to the first reaction product obtained in step 1) in sequence to react to obtain a second reaction product;
[0022] 3) adding sodium montmorillonite to the second reaction product obtained in step 2) to carry out an intercalation reaction to obtain a third reaction product;
[0023] 4) The third reaction product obtained in step 3) is centrifuged, precipitated, washed, dried, and crushed to obtain a light yellow powder, which is the organic-inorganic hybrid core material.
[0024] As a specific embodiment of the present invention, in the step 1), the dissolution conditions include: a temperature of 80°C to 95°C, a stirring speed of 200rpm to 400rpm, and a stirring time of 30min to 60min; the solvent is water, and the solvent is 1-1.5 times the mass of the polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer;
[0025] As a specific embodiment of the present invention, in the step 2), the reaction conditions include: a stirring speed of 1000 rpm to 3000 rpm, and a reaction time of 30 min to 60 min;
[0026] As a specific embodiment of the present invention, in the step 3), the intercalation reaction conditions include: a stirring speed of 100 rpm to 500 rpm, and a reaction time of 80 min to 120 min;
[0027] As a specific embodiment of the present invention, in the step 4), the centrifugal conditions include: a centrifugal rate of 15000 rpm to 30000 rpm, a centrifugal time of 15 to 20 min, the washing until the pH of the leached liquid is 6.8 to 7.0; and the crushing to 1000 mesh.
[0028] As a specific embodiment of the present invention, the molecular formula of the polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer is PEOm-PPOn-PEOm, m is preferably 200-1000, n is preferably 50-250, and the number average molecular weight is preferably 20000-120000.
[0029] As a specific embodiment of the present invention, the nano nucleating agent is one of nano calcium carbonate, nano silicon dioxide, and nano iron oxide, or a combination of any two thereof, and the particle size is preferably 100 nm to 120 nm.
[0030] As a specific embodiment of the present invention, the alkali provider is one or a combination of any two of sodium hydroxide, sodium carbonate, sodium bicarbonate, and sodium silicate.
[0031] As a specific embodiment of the present invention, the sodium montmorillonite is a layered silicate mineral, the basic units of which are silicon-oxygen tetrahedron and aluminum-oxygen octahedron, with a flaky and layered structure, a flaky layer thickness of 1 to 3 nm, and a flaky layer width of 200 to 600 nm.
[0032] Exemplarily, the method for preparing the organic-inorganic hybrid core material comprises the following steps:
[0033] 1) Add 400g to 800g of polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer and 500g to 1000g of deionized water into an autoclave, raise the system temperature to 80°C to 95°C, adjust the stirring speed to 200rpm to 400rpm, and dissolve for 30min to 60min;
[0034] 2) Slowly add 50g to 100g of nano nucleating agent into the above reactor, increase the stirring speed to 1000rpm to 3000rpm, add the whole amount within 10min to 30min, and continue the reaction for 30min to 60min after the addition;
[0035] 3) 4000 g to 8000 g of deionized water and 20 g to 50 g of an alkali provider were quickly added to the reactor in sequence, and stirred for 30 min to 60 min;
[0036] 4) Slowly add 1200g to 2400g of sodium montmorillonite into the above reactor, reduce the stirring speed to 100rpm to 500rpm, and perform intercalation reaction for 80min to 120min;
[0037] 5) After the reaction is completed, transfer to a centrifuge and centrifuge at 15000 rpm to 30000 rpm for 20 min. Collect the precipitate and wash it several times with deionized water until the pH of the leached liquid is 6.8 to 7.0;
[0038] 6) The collected final precipitate is dried, crushed, and passed through a 1000-mesh sieve to obtain a light yellow powder, which is the organic-inorganic hybrid core material.
[0039] In a second aspect, the present invention provides a method for preparing the energy storage medium according to the first aspect, comprising the following steps:
[0040] S1: mixing deionized water and a thickener to obtain a swollen thickener;
[0041] S2: Add the organic-inorganic hybrid core material / alginate microspheres to the swollen viscosity enhancer obtained in step S1 and mix them evenly to obtain an energy storage medium.
[0042] As a specific embodiment of the present invention, in step S1, the mixing conditions include: mixing temperature of 60°C to 80°C; stirring speed of 500rpm to 1000rpm, stirring time of 30min to 60min;
[0043] As a specific embodiment of the present invention, in step S2, the mixing conditions include: a stirring speed of 2000 rpm to 4000 rpm, and a stirring time of 30 min to 60 min.
[0044] Exemplarily, the method for preparing the energy storage medium comprises the following steps:
[0045] 1) Add 2000 g to 6000 g of deionized water into the autoclave and raise the system temperature to 60° C. to 80° C.;
[0046] 2) Add 30g to 40g of viscosity enhancer into the above reactor, set the stirring speed to 500rpm to 1000rpm, and allow the solution to swell and increase viscosity for 30min to 60min;
[0047] 3) Add 1500g to 5000g of organic-inorganic hybrid core material / alginate microspheres into the above reactor, adjust the stirring speed to 2000rpm to 4000rpm, and disperse for 30min to 60min;
[0048] 4) After the reaction is completed, the obtained suspension system is the energy storage medium for rapid cooling.
[0049] The above raw materials in the present invention can be prepared in-house or commercially available, and the present invention is not particularly limited thereto.
[0050] In a third aspect, the present invention provides an application of the energy storage medium described in the first aspect or the energy storage medium prepared by the preparation method described in the second aspect in the field of rapid cooling of drilling fluid surface.
[0051] Compared with the prior art, the present invention has the following beneficial effects:
[0052] 1. The energy storage medium of the present invention uses an organic-inorganic hybrid intercalation method to insert a block copolymer into an inorganic montmorillonite layer, thereby improving the stability of the polymer during hot melting and reducing the defect of the currently used energy storage material that is easy to deform and thus leads to poor stability.
[0053] 2. The energy storage medium of the present invention adopts the method of encapsulating alginate into microspheres to improve its dispersion and flow effect in the fluid, and the system has a higher energy storage effect.
[0054] 3. The energy storage medium of the present invention can greatly improve the heat absorption efficiency and achieve the purpose of rapid cooling. DETAILED DESCRIPTION
[0055] The present invention will be further described below in conjunction with specific embodiments, but they do not constitute any limitation to the present invention.
[0056] The sodium montmorillonite flakes used in the following embodiments of the present invention have a thickness of 1 to 3 nm and a width of 200 to 600 nm. They are produced in Xiazijie, Xinjiang and purchased from Xinjiang Central Africa Xiazijie Bentonite Co., Ltd.
[0057] Example 1
[0058] This embodiment provides an energy storage medium and a preparation method thereof, the specific details of which are as follows:
[0059] Preparation of organic-inorganic hybrid core material:
[0060] 1) Add 400 g of polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer (PEO 200 -PPO 50 -PEO 200 , number average molecular weight is 20500) and 500g deionized water, raise the system temperature to 80°C, adjust the stirring speed to 200rpm, and dissolve for 30min;
[0061] 2) Slowly add 50g of nano calcium carbonate into the above reactor, increase the stirring speed to 1000rpm, add it within 10min, and continue to react for 30min after adding;
[0062] 3) 4000 g of deionized water and 20 g of sodium hydroxide were quickly added to the above reactor in sequence and stirred for 30 min;
[0063] 4) Slowly add 1200 g of sodium montmorillonite into the above reactor, reduce the stirring speed to 100 rpm, and perform intercalation reaction for 80 min;
[0064] 5) After the reaction is completed, transfer to a centrifuge and centrifuge at 15,000 rpm for 20 min. Collect the precipitate and wash it several times with deionized water until the pH of the leached liquid is 6.8;
[0065] 6) The collected final precipitate is dried, crushed, and passed through a 1000-mesh sieve to obtain a light yellow powder, which is the organic-inorganic hybrid core material.
[0066] Preparation of organic-inorganic hybrid core material / alginate microspheres:
[0067] 1) In a closed autoclave, 800 g of organic-inorganic hybrid core material, 1600 g of sodium alginate and 3000 g of deionized water were added in sequence, the system temperature was raised to 70°C, the stirring speed was adjusted to 1000 rpm, and the mixture was stirred and dispersed for 30 min;
[0068] 2) Add 400g of calcium chloride to the above reactor, reduce the stirring speed to 100rpm, and solidify into balls for 12h;
[0069] 3) After the reaction is completed, the generated microspheres are fished out and washed three times with deionized water, and the millimeter-sized microspheres are screened out by centrifugal screening;
[0070] 4) The system was then transferred to a rotary evaporator to remove the remaining solvent. The obtained microspheres were organic-inorganic hybrid core material / alginate microspheres with an average diameter of 1.5 mm, an average wall thickness of 0.3 mm, and a mass percentage of organic-inorganic hybrid core material to microspheres of 85%.
[0071] Energy storage medium preparation:
[0072] 1) Add 2000 g of deionized water into the autoclave and raise the system temperature to 60°C;
[0073] 2) Add 30 g of polyacrylamide (number average molecular weight 500×10 4 ), set the stirring speed to 500 rpm, and allow swelling and viscosity increasing for 30 min;
[0074] 3) Add 1500g of organic-inorganic hybrid core material / alginate microspheres into the above reactor, adjust the stirring speed to 2000rpm, and disperse for 30min;
[0075] 4) After the reaction is completed, the obtained suspension system is the energy storage medium.
[0076] The energy storage medium obtained in Example 1 contains 56.66% deionized water, 0.85% viscosity enhancer, and 42.49% organic-inorganic hybrid core material / alginate microspheres.
[0077] Example 2
[0078] This embodiment provides an energy storage medium and a preparation method thereof, the specific details of which are as follows:
[0079] Preparation of organic-inorganic hybrid core material:
[0080] 1) Add 500 g of polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer (PEO 400 -PPO 80 -PEO 400 , number average molecular weight 39840) and 600g deionized water, raise the system temperature to 85°C, adjust the stirring speed to 300rpm, and dissolve for 40min;
[0081] 2) Slowly add 60g of nano-silicon dioxide into the above reactor, increase the stirring speed to 2000rpm, add it within 20min, and continue the reaction for 40min after the addition;
[0082] 3) 5000 g of deionized water and 30 g of sodium carbonate were quickly added to the above reactor in sequence and stirred for 40 min;
[0083] 4) Slowly add 1500 g of sodium montmorillonite into the above reactor, reduce the stirring speed to 200 rpm, and perform intercalation reaction for 90 min;
[0084] 5) After the reaction is completed, transfer to a centrifuge and centrifuge at 17,000 rpm for 20 min. Collect the precipitate and wash it several times with deionized water until the pH of the leached liquid is 6.85;
[0085] 6) The collected final precipitate is dried, crushed, and passed through a 1000-mesh sieve to obtain a light yellow powder, which is the organic-inorganic hybrid core material.
[0086] Preparation of organic-inorganic hybrid core material / alginate microspheres:
[0087] 1) Add 900 g of organic-inorganic hybrid core material, 1800 g of sodium alginate and 3100 g of deionized water in a closed autoclave, raise the system temperature to 80° C., adjust the stirring speed to 2000 rpm, and stir and disperse for 40 min;
[0088] 2) Add 500g of calcium bromide to the above reactor, reduce the stirring speed to 200rpm, and solidify into balls for 16h;
[0089] 3) After the reaction is completed, the generated microspheres are fished out and washed three times with deionized water, and the millimeter-sized microspheres are screened out by centrifugal screening;
[0090] 4) The system was then transferred to a rotary evaporator to remove the remaining solvent, and the obtained microspheres were organic-inorganic hybrid core material / alginate microspheres with an average diameter of 2.5 mm, an average wall thickness of 0.5 mm, and a mass percentage of organic-inorganic hybrid core material to microspheres of 88%.
[0091] Energy storage medium preparation:
[0092] 1) Add 3000 g of deionized water into the autoclave and raise the system temperature to 70°C;
[0093] 2) Add 35 g of hydroxymethyl cellulose (number average molecular weight 600×10 4 ), set the stirring speed to 600 rpm, and allow swelling and viscosity increasing for 40 min;
[0094] 3) Add 1800 g of organic-inorganic hybrid core material / alginate microspheres into the above reactor, adjust the stirring speed to 3000 rpm, and disperse for 40 min;
[0095] 4) After the reaction is completed, the obtained suspension system is the energy storage medium.
[0096] The energy storage medium obtained in Example 2 contains 62.05% deionized water, 0.72% viscosity enhancer, and 37.23% organic-inorganic hybrid core material / alginate microspheres.
[0097] Example 3
[0098] This embodiment provides an energy storage medium and a preparation method thereof, the specific details of which are as follows:
[0099] Preparation of organic-inorganic hybrid core material:
[0100] 1) Add 600 g of polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer (PEO 600 -PPO 100 -PEO 600 , number average molecular weight of 58600) and 700g of deionized water, raise the system temperature to 95°C, adjust the stirring speed to 400rpm, and dissolve for 50min;
[0101] 2) Slowly add 700g of nano iron oxide into the above reactor, increase the stirring speed to 3000rpm, add it within 30min, and continue the reaction for 50min after the addition;
[0102] 3) 6000 g of deionized water and 40 g of sodium bicarbonate were quickly added to the above reactor in sequence and stirred for 50 min;
[0103] 4) Slowly add 1600 g of sodium montmorillonite into the above reactor, reduce the stirring speed to 200 rpm, and perform intercalation reaction for 100 min;
[0104] 5) After the reaction is completed, transfer to a centrifuge and centrifuge at 19000 rpm for 20 min. Collect the precipitate and wash it several times with deionized water until the pH of the leached liquid is 6.9;
[0105] 6) The collected final precipitate is dried, crushed, and passed through a 1000-mesh sieve to obtain a light yellow powder, which is the organic-inorganic hybrid core material.
[0106] Preparation of organic-inorganic hybrid core material / alginate microspheres:
[0107] 1) Add 1000 g of organic-inorganic hybrid core material, 1900 g of sodium alginate and 3200 g of deionized water in a closed autoclave, raise the system temperature to 90° C., adjust the stirring speed to 3000 rpm, and stir and disperse for 50 min;
[0108] 2) Add 600 g of calcium nitrate to the above reactor, reduce the stirring speed to 300 rpm, and solidify into balls for 16 hours;
[0109] 3) After the reaction is completed, the generated microspheres are fished out and washed three times with deionized water, and the millimeter-sized microspheres are screened out by centrifugal screening;
[0110] 4) The system was then transferred to a rotary evaporator to remove the remaining solvent, and the obtained microspheres were organic-inorganic hybrid core material / alginate microspheres with an average diameter of 4.5 mm, an average wall thickness of 0.7 mm, and a mass percentage of organic-inorganic hybrid core material to microspheres of 90.8%.
[0111] Energy storage medium preparation:
[0112] 1) Add 4000 g of deionized water into the autoclave and raise the system temperature to 80°C;
[0113] 2) Add 40 g of carboxymethyl starch (number average molecular weight 700×10 4 ), set the stirring speed to 700 rpm, and allow swelling and viscosity increasing for 50 min;
[0114] 3) Add 2000 g of organic-inorganic hybrid core material / alginate microspheres into the above reactor, adjust the stirring speed to 4000 rpm, and disperse for 50 min;
[0115] 4) After the reaction is completed, the obtained suspension system is the energy storage medium.
[0116] The energy storage medium obtained in Example 3 contains 66.23% deionized water, 0.66% viscosity enhancer, and 33.11% organic-inorganic hybrid core material / alginate microspheres.
[0117] Example 4
[0118] This embodiment provides an energy storage medium and a preparation method thereof, the specific details of which are as follows:
[0119] Preparation of organic-inorganic hybrid core material:
[0120] 1) Add 700 g of polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer (PEO 800 -PPO 120 -PEO 800 , number average molecular weight 77360) and 800g deionized water, raise the system temperature to 95°C, adjust the stirring speed to 400rpm, and dissolve for 60min;
[0121] 2) Slowly add 800g of nano calcium carbonate into the above reactor, increase the stirring speed to 3000rpm, add it within 30min, and continue the reaction for 60min after the addition;
[0122] 3) Quickly add 7000g of deionized water and 50g of sodium silicate into the above reactor in sequence and stir thoroughly for 60min;
[0123] 4) Slowly add 1800 g of sodium montmorillonite into the above reactor, reduce the stirring speed to 400 rpm, and perform intercalation reaction for 120 min;
[0124] 5) After the reaction is completed, transfer to a centrifuge and centrifuge at 20,000 rpm for 20 min. Collect the precipitate and wash it several times with deionized water until the pH of the leached liquid is 6.8;
[0125] 6) The collected final precipitate is dried, crushed, and passed through a 1000-mesh sieve to obtain a light yellow powder, which is the organic-inorganic hybrid core material.
[0126] Preparation of organic-inorganic hybrid core material / alginate microspheres:
[0127] 1) Add 1500g of organic-inorganic hybrid core material, 2000g of sodium alginate and 3500g of deionized water in a closed autoclave, raise the system temperature to 90°C, adjust the stirring speed to 3000rpm, and stir and disperse for 60min;
[0128] 2) Add 700g of calcium chloride to the above reactor, reduce the stirring speed to 400rpm, and solidify into balls for 24h;
[0129] 3) After the reaction is completed, the generated microspheres are fished out and washed three times with deionized water, and the millimeter-sized microspheres are screened out by centrifugal screening;
[0130] 4) The system was then transferred to a rotary evaporator to remove the remaining solvent, and the obtained microspheres were organic-inorganic hybrid core material / alginate microspheres with an average diameter of 5.0 mm, an average wall thickness of 0.7 mm, and a mass percentage of organic-inorganic hybrid core material to microspheres of 92.0%.
[0131] Energy storage medium preparation:
[0132] 1) Add 5000 g of deionized water into the autoclave and raise the system temperature to 80°C;
[0133] 2) Add 40 g of carboxymethyl starch (number average molecular weight 800×10 4 ), set the stirring speed to 8000 rpm, and allow swelling and viscosity increasing for 60 min;
[0134] 3) Add 3000 g of organic-inorganic hybrid core material / alginate microspheres into the above reactor, adjust the stirring speed to 4000 rpm, and disperse for 60 min;
[0135] 4) After the reaction is completed, the obtained suspension system is the energy storage medium.
[0136] The energy storage medium obtained in Example 4 contains 62.19% deionized water, 0.50% viscosity enhancer, and 37.31% organic-inorganic hybrid core material / alginate microspheres.
[0137] Example 5
[0138] This embodiment provides an energy storage medium and a preparation method thereof, the specific details of which are as follows:
[0139] Preparation of organic-inorganic hybrid core material:
[0140] 1) Add 800 g of polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer (PEO 1000 -PPO 180 -PEO 1000 , number average molecular weight 98440) and 900g deionized water, raise the system temperature to 95°C, adjust the stirring speed to 400rpm, and dissolve for 60min;
[0141] 2) Slowly add 900g of nano-silicon dioxide into the above reactor, increase the stirring speed to 3000rpm, add it within 30min, and continue the reaction for 60min after the addition;
[0142] 3) 8000 g of deionized water and 50 g of sodium hydroxide were quickly added to the above reactor in sequence and stirred for 60 min;
[0143] 4) Slowly add 2200 g of sodium montmorillonite into the above reactor, reduce the stirring speed to 500 rpm, and perform intercalation reaction for 120 min;
[0144] 5) After the reaction is completed, transfer to a centrifuge and centrifuge at 24,000 rpm for 20 min. Collect the precipitate and wash it several times with deionized water until the pH of the leached liquid is 6.95;
[0145] 6) The collected final precipitate is dried, crushed, and passed through a 1000-mesh sieve to obtain a light yellow powder, which is the organic-inorganic hybrid core material.
[0146] Preparation of organic-inorganic hybrid core material / alginate microspheres:
[0147] 1) Add 1200 g of organic-inorganic hybrid core material, 2000 g of sodium alginate and 3500 g of deionized water in a closed autoclave, raise the system temperature to 90° C., adjust the stirring speed to 3000 rpm, and stir and disperse for 60 min;
[0148] 2) Add 800g of calcium bromide to the above reactor, reduce the stirring speed to 500rpm, and solidify into balls for 24h;
[0149] 3) After the reaction is completed, the generated microspheres are fished out and washed three times with deionized water, and the millimeter-sized microspheres are screened out by centrifugal screening;
[0150] 4) The system was then transferred to a rotary evaporator to remove the remaining solvent, and the obtained microspheres were organic-inorganic hybrid core material / alginate microspheres with an average diameter of 1.9 mm, an average wall thickness of 0.2 mm, and a mass percentage of organic-inorganic hybrid core material to microspheres of 88.3%.
[0151] Energy storage medium preparation:
[0152] 1) Add 6000 g of deionized water into the autoclave and raise the system temperature to 0°C;
[0153] 2) Add 40 g of hydroxymethyl cellulose (number average molecular weight 900×10 4 ), set the stirring speed to 1000 rpm, and allow swelling and viscosity increasing for 360 min;
[0154] 3) Add 5000 g of organic-inorganic hybrid core material / alginate microspheres into the above reactor, adjust the stirring speed to 4000 rpm, and disperse for 360 min;
[0155] 4) After the reaction is completed, the obtained suspension system is the energy storage medium.
[0156] The energy storage medium obtained in Example 5 contains 54.35% deionized water, 0.36% viscosity enhancer, and 45.29% organic-inorganic hybrid core material / alginate microspheres.
[0157] Example 6
[0158] This embodiment provides an energy storage medium and a preparation method thereof, the specific details of which are as follows:
[0159] Preparation of organic-inorganic hybrid core material:
[0160] 1) Add 800 g of polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer (PEO 1000 -PPO 200 -PEO 1000 , number average molecular weight is 99600) and 1000g deionized water, raise the system temperature to 95°C, adjust the stirring speed to 400rpm, and dissolve for 60min;
[0161] 2) Slowly add 100g of nano iron oxide into the above reactor, increase the stirring speed to 3000rpm, add it within 30min, and continue the reaction for 60min after the addition;
[0162] 3) Quickly add ~8000 g of deionized water and 50 g of sodium carbonate into the above reactor in sequence and stir thoroughly for 60 min;
[0163] 4) Slowly add 2400 g of sodium montmorillonite into the above reactor, reduce the stirring speed to 500 rpm, and perform intercalation reaction for 120 min;
[0164] 5) After the reaction is completed, transfer to a centrifuge and centrifuge at 30,000 rpm for 20 min. Collect the precipitate and wash it several times with deionized water until the pH of the leached liquid is 6.9;
[0165] 6) The collected final precipitate is dried, crushed, and passed through a 1000-mesh sieve to obtain a light yellow powder, which is the organic-inorganic hybrid core material.
[0166] Preparation of organic-inorganic hybrid core material / alginate microspheres:
[0167] 1) Add 1500g of organic-inorganic hybrid core material, 2000g of sodium alginate and 3500g of deionized water in a closed autoclave, raise the system temperature to 90°C, adjust the stirring speed to 3000rpm, and stir and disperse for 60min;
[0168] 2) Add 800g of calcium nitrate to the above reactor, reduce the stirring speed to 500rpm, and solidify into balls for 24h;
[0169] 3) After the reaction is completed, the generated microspheres are fished out and washed three times with deionized water, and the millimeter-sized microspheres are screened out by centrifugal screening;
[0170] 4) The system was then transferred to a rotary evaporator to remove the remaining solvent, and the obtained microspheres were organic-inorganic hybrid core material / alginate microspheres with an average diameter of 3.5 mm, an average wall thickness of 0.2 mm, and a mass percentage of organic-inorganic hybrid core material to microspheres of 86.4%.
[0171] Energy storage medium preparation:
[0172] 1) Add 6000 g of deionized water into the autoclave and raise the system temperature to 80°C;
[0173] 2) Add 40 g of carboxymethyl starch (number average molecular weight 1000×10 4 ), set the stirring speed to 1000 rpm, and allow swelling and viscosity increasing for 60 min;
[0174] 3) Add 5000 g of organic-inorganic hybrid core material / alginate microspheres into the above reactor, adjust the stirring speed to 4000 rpm, and disperse for 60 min;
[0175] 4) After the reaction is completed, the obtained suspension system is the energy storage medium.
[0176] The energy storage medium obtained in Example 6 contains 54.35% deionized water, 0.36% viscosity enhancer, and 45.29% organic-inorganic hybrid core material / alginate microspheres.
[0177] Example 7
[0178] This embodiment provides an energy storage medium and a preparation method thereof, the specific details of which are as follows:
[0179] Preparation of organic-inorganic hybrid core material:
[0180] 1) Add 800 g of polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer (PEO 1000 -PPO 250 -PEO 1000, number average molecular weight of 102500) and 950g of deionized water, raise the system temperature to 95°C, adjust the stirring speed to 400rpm, and dissolve for 60min;
[0181] 2) Slowly add 100g of nano calcium carbonate into the above reactor, increase the stirring speed to 3000rpm, add it within 30min, and continue the reaction for 60min after the addition;
[0182] 3) 8000 g of deionized water and 50 g of sodium bicarbonate were quickly added to the above reactor in sequence and stirred for 60 min;
[0183] 4) Slowly add 2400 g of sodium montmorillonite into the above reactor, reduce the stirring speed to 500 rpm, and perform intercalation reaction for 120 min;
[0184] 5) After the reaction is completed, transfer to a centrifuge and centrifuge at 30,000 rpm for 20 min. Collect the precipitate and wash it several times with deionized water until the pH of the leached liquid is 6.8;
[0185] 6) The collected final precipitate is dried, crushed, and passed through a 1000-mesh sieve to obtain a light yellow powder, which is the organic-inorganic hybrid core material.
[0186] Preparation of organic-inorganic hybrid core material / alginate microspheres:
[0187] 1) Add 1500g of organic-inorganic hybrid core material, 2000g of sodium alginate and 3500g of deionized water in a closed autoclave, raise the system temperature to 70°C to 90°C, adjust the stirring speed to 3000rpm, and stir and disperse for 60min;
[0188] 2) Add 800g of calcium chloride to the above reactor, reduce the stirring speed to 500rpm, and solidify into balls for 24h;
[0189] 3) After the reaction is completed, the generated microspheres are fished out and washed three times with deionized water, and the millimeter-sized microspheres are screened out by centrifugal screening;
[0190] 4) The system was then transferred to a rotary evaporator to remove the remaining solvent, and the obtained microspheres were organic-inorganic hybrid core material / alginate microspheres with an average diameter of 3.7 mm, an average wall thickness of 0.2 mm, and a mass percentage of organic-inorganic hybrid core material to microspheres of 90.5%.
[0191] Energy storage medium preparation:
[0192] 1) Add 6000 g of deionized water into the autoclave and raise the system temperature to 80°C;
[0193] 2) Add ~40 g of polyacrylamide (number average molecular weight 600×10 4 ), set the stirring speed to 1000 rpm, and allow swelling and viscosity increasing for 60 min;
[0194] 3) Add 5000 g of organic-inorganic hybrid core material / alginate microspheres into the above reactor, adjust the stirring speed to 4000 rpm, and disperse for 60 min;
[0195] 4) After the reaction is completed, the obtained suspension system is an energy storage medium.
[0196] The energy storage medium obtained in Example 7 contains 54.35% deionized water, 0.36% viscosity enhancer, and 45.29% organic-inorganic hybrid core material / alginate microspheres.
[0197] Test Case
[0198] (1) Phase transition temperature test: The DSC curve is obtained by measuring the heating curve and the cooling curve. According to the regulations of the ICTA Standardization Committee, the upward DSC curve is an exothermic peak and the downward DSC curve is an endothermic peak. The intersection of the extension line of the front baseline and the tangent line at the maximum slope of the peak front is the melting point. The crystallization peak of melting and recrystallization is taken as the characteristic peak for analysis to obtain the phase transition temperature, phase transition latent heat and other thermophysical parameters.
[0199] (2) Cooling efficiency test: Hot water (90°C, pipe diameter 10 cm, displacement 30 L / s) is passed through the pipes used. The condenser is arranged in a winding manner. Different fluids are passed through the pipes to test the temperature difference between the inlet and outlet of the pipes. The cooling efficiency is obtained by dividing the temperature difference by the initial temperature.
[0200] This test example tests the phase change temperature and cooling efficiency of the energy storage medium obtained in Examples 1-7, and compares them with conventional water cooling and air cooling. The results are shown in Table 1.
[0201] Table 1 Phase transition temperature and cooling efficiency of different systems
[0202]
[0203]
[0204] From the results in Table 1, it can be seen that the cooling effects of conventional water cooling and air cooling are both lower than 15.0%, while the use of energy storage medium can greatly improve the cooling effect of the system, and the cooling efficiency exceeds 27.0%, achieving a better cooling effect.
[0205] In summary, the energy storage medium of the present invention mainly adopts an organic-inorganic hybrid method to form a composite energy storage material, and is encapsulated by an alginate microcapsule method to form a high-efficiency energy storage material. The purpose of quickly reducing the temperature of the drilling fluid can be achieved by density cycling of high-concentration energy storage materials.
[0206] Any numerical value mentioned in the present invention, if there is only an interval of two units between any minimum value and any maximum value, includes all values from the minimum value to the maximum value each time increasing by one unit. For example, if the amount of a component, or the value of a process variable such as temperature, pressure, time, etc. is declared to be 50-90, in this specification it means that 51-89, 52-88... and 69-71 and 70-71 are specifically listed. For non-integer values, 0.1, 0.01, 0.001 or 0.0001 can be appropriately considered as a unit. These are just some specially specified examples. In this application, in a similar manner, all possible combinations of numerical values between the listed minimum and maximum values are considered to have been disclosed.
[0207] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.
Claims
1. An energy storage medium, characterized in that: The energy storage medium comprises, by mass percentage, 50% to 70% of deionized water, 0.2% to 5.0% of a viscosity enhancer, and 40% to 50% of an organic-inorganic hybrid core material / alginate microspheres.
2. The energy storage medium according to claim 1, characterized in that The thickener comprises one or any combination of polyacrylamide, hydroxymethyl cellulose and carboxymethyl starch, and / or the number average molecular weight of the thickener is 500×10 4 ~1000×10 4 .
3. The energy storage medium according to claim 1 or 2, characterized in that: The diameter of the organic-inorganic hybrid core material / alginate microspheres is 1 mm to 5 mm, the wall thickness is 0.1 mm to 0.5 mm, and the mass percentage of the organic-inorganic hybrid core material to the microspheres is 80% to 92%.
4. The energy storage medium according to any one of claims 1 to 3, characterized in that: The preparation method of the organic-inorganic hybrid core material / alginate microspheres comprises: reacting and curing the organic-inorganic hybrid core material and sodium alginate under the action of a curing agent.
5. The energy storage medium according to claim 4, characterized in that The reaction conditions include: temperature of 70°C to 90°C, stirring speed of 1000rpm to 3000rpm, and reaction time of 30min to 60min; the curing conditions include: stirring speed of 100rpm to 500rpm, and curing time of 12h to 24h; The curing agent is one of calcium chloride, calcium bromide and calcium nitrate or a combination of any two thereof.
6. The energy storage medium according to any one of claims 1 to 5, characterized in that: The raw materials for preparing the organic-inorganic hybrid core material include polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer, nano nucleating agent, alkali providing agent and sodium montmorillonite; Preferably, the preparation of the organic-inorganic hybrid core material comprises the following steps: 1) adding a nano nucleating agent to the dissolved polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer to react to obtain a first reaction product; 2) adding deionized water and an alkali provider to the first reaction product obtained in step 1) in sequence to react to obtain a second reaction product; 3) adding sodium montmorillonite to the second reaction product obtained in step 2) to carry out an intercalation reaction to obtain a third reaction product; 4) The third reaction product obtained in step 3) is centrifuged, precipitated, washed, dried, and crushed to obtain a light yellow powder, which is the organic-inorganic hybrid core material. More preferably, in the step 1), the dissolution conditions include: a temperature of 80°C to 95°C, a stirring speed of 200rpm to 400rpm, and a stirring time of 30min to 60min; the solvent is water; and the solvent is 1 to 1.5 times the mass of the polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer; In the step 2), the reaction conditions include: a stirring speed of 1000 rpm to 3000 rpm, and a reaction time of 30 min to 60 min; In the step 3), the intercalation reaction conditions include: a stirring speed of 100 rpm to 500 rpm, and a reaction time of 80 min to 120 min; In the step 4), the centrifugal conditions include: a centrifugal rate of 15000 rpm to 30000 rpm, a centrifugal time of 15 to 20 min, the washing until the pH of the leached liquid is 6.8 to 7.0; and the crushing to 1000 mesh.
7. The energy storage medium according to any one of claims 1 to 6, characterized in that: The molecular formula of the polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer is PEOm-PPOn-PEOm, m is preferably 200 to 1000, n is preferably 50 to 250, and the number average molecular weight is preferably 20000 to 120000; and / or, The nano nucleating agent is one of nano calcium carbonate, nano silicon dioxide, nano iron oxide or any combination of two thereof, and the particle size is preferably 100nm to 120nm; and / or, the alkali providing agent is one of sodium hydroxide, sodium carbonate, sodium bicarbonate or sodium silicate or any combination of two thereof; and / or, The sodium-based montmorillonite is a layered silicate mineral, the basic units of which are silicon-oxygen tetrahedron and aluminum-oxygen octahedron, and has a flaky and layered structure, a flaky layer thickness of 1 to 3 nm, and a flaky layer width of 200 to 600 nm.
8. The method for preparing the energy storage medium according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1: mixing deionized water and a thickener to obtain a swollen thickener; S2: Add the organic-inorganic hybrid core material / alginate microspheres to the swollen viscosity enhancer obtained in step S1 and mix them evenly to obtain an energy storage medium.
9. The preparation method according to claim 8, characterized in that: In step S1, the mixing conditions include: a mixing temperature of 60°C to 80°C; a stirring speed of 500rpm to 1000rpm, and a stirring time of 30min to 60min; and / or, In step S2, the mixing conditions include: a stirring speed of 2000 rpm to 4000 rpm, and a stirring time of 30 min to 60 min.
10. Use of the energy storage medium according to any one of claims 1 to 7 or the energy storage medium prepared by the preparation method according to claim 8 or 9 in the field of rapid cooling of drilling fluid surface.