Self-consolidation plugging agent and application thereof
Through a self-consolidation leak plugging agent combined with thermosetting resin and inorganic composite materials, the sealing problem of malignant leakage in oil and gas wells is solved, and efficient leak plugging effect and safe production are achieved.
Patent Information
- Application Number
- CN202310603319.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-26
AI Technical Summary
The well leakage problem caused by vicious leakage in oil and gas well exploration lacks effective sealing technology, which leads to problems such as buried drilling and well collapse. The existing thermosetting resin has high viscosity at room temperature and is difficult to pump.
A combination of thermosetting resin, inorganic composite materials, silane coupling agent, dicyanide diamine, dimethylimidazole and amide compounds is used to prepare a self-consolidation plugging agent with good room temperature flowability and pumpability, and It cures at 150℃, has high compressive strength, and can effectively seal large cracks.
It achieves good flowability and pumpability at room temperature, controllable consolidation time, high compressive strength, can effectively seal large cracks, and is insoluble under high temperature conditions, has complete structure, and has significant advantages in malignant leakage management. .
Smart Images

Figure CN119020005A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of cementing and plugging, and in particular to a self-consolidating plugging agent. Background Art
[0002] In the exploration and development of oil and gas wells, the problem of well leakage is a technical problem that troubles the world. The number of well leakages in the world accounts for 20% to 25% of the total. The losses caused by well leakage are as high as hundreds of millions of dollars every year, which brings immeasurable losses to the development of oil and gas wells. The problem of malignant leakage caused by cave leakage and large fracture leakage has seriously restricted the exploration and development of oil and gas wells. There is still no good plugging technology for malignant leakage at home and abroad, which may eventually lead to buried drilling, well collapse and even become scrapped wells. Summary of the invention
[0003] One of the present inventions provides a self-consolidating plugging agent, which comprises a thermosetting resin, an inorganic composite material, a silane coupling agent, dicyandiamide, dimethylimidazole and an amide compound.
[0004] In a specific embodiment, the epoxy value of the thermosetting resin is above 0.44.
[0005] In a specific embodiment, the thermosetting resin is thermosetting resin E44.
[0006] In a specific embodiment, the inorganic composite material is calcium carbonate and glass fiber.
[0007] In a specific embodiment, the mass ratio of the calcium carbonate to the glass fiber is (5 to 8):3.
[0008] In a specific embodiment, the particle size of the calcium carbonate is 800 to 1200 mesh; the length of the glass fiber is 0.2 to 0.6 mm.
[0009] In a specific embodiment, the silane coupling agent is silane coupling agent KH550.
[0010] In a specific embodiment, the amide compound is dimethylacetamide (DMA) and / or dimethylformamide (DMF).
[0011] In a specific embodiment, the mass ratio of the thermosetting resin to the inorganic composite material is (8.1 to 19):1.
[0012] In a specific embodiment, the mass ratio of the thermosetting resin to the amide compound is (4 to 5):1.
[0013] In a specific embodiment, the mass ratio of the thermosetting resin, the dicyandiamide and the dimethylimidazole is 100:(6 to 10):(0.2 to 0.6).
[0014] In a specific embodiment, based on the total mass of the inorganic composite material being 100%, the mass of the silane coupling agent is 2% to 4% of the inorganic composite material.
[0015] The second aspect of the present invention provides a method for preparing the self-consolidating plugging agent as described in any one of the first aspect of the present invention, which comprises the following steps:
[0016] 1) dissolving dicyandiamide and dimethylimidazole in an amide compound to obtain a first mixed solution;
[0017] 2) adding a thermosetting resin into the first mixed solution and mixing them evenly to obtain a second mixed solution;
[0018] 3) adding a silane coupling agent to the second mixed solution and mixing them evenly to obtain a third mixed solution;
[0019] 4) adding the inorganic composite material to the third mixed liquid and mixing them evenly to obtain the self-consolidating plugging agent.
[0020] The third aspect of the present invention provides the use of the self-consolidating plugging agent according to any one of the present inventions in plugging leaks in oil and gas drilling.
[0021] Beneficial effects of the present invention:
[0022] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a controllable self-consolidating plugging agent for plugging a vicious leakage formation and a preparation method thereof.
[0023] The present invention solves the problem that thermosetting resins have high viscosity and are difficult to pump at room temperature, so that the controllable self-consolidating plugging agent of the present invention has good fluidity and pumpability at room temperature, and thus has room temperature pumpability; its temperature resistance can reach 150°C, and the consolidation time is controllable within the range of 0.5h to 4.5h, especially controllable within the range of 1.2 to 2.5h, so it has temperature controllability of the consolidation time, and the self-consolidating plugging agent of the present invention has high consolidation compressive strength, which is greater than 40MPa, and good pressure-bearing plugging property for plugging 1cm cracks, and a breakthrough pressure gradient of greater than 85MPa / m, so it can effectively plug large cracks such as 1cm, and has obvious advantages in the technology of malignant leakage control.
[0024] In addition, the self-consolidating plugging agent of the present invention has a drillability of grade five to grade six after solidification, and has good drillability; when placed in water-based drilling fluid and simulated formation water, it does not dissolve or deform at 150°C, has a complete structure, and has good anti-pollution properties. It can be effectively dissolved by an environmentally friendly solvent in the later stage to achieve the purpose of unblocking, avoiding wellbore blockage and causing production safety accidents, and has achieved significant new breakthroughs in conventional malignant leakage control technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The solidified product 6# of the plugging agent prepared in Example 6 is shown.
[0026] Figure 2 The state of the solidified product 6# of the plugging agent prepared in Example 6 after being dissolved in the dissolving agent GY-1 for 2 hours is shown.
[0027] Figure 3 The state of the solidified product 6# of the plugging agent prepared in Example 6 after being dissolved in the dissolving agent GY-1 for 8 hours is shown.
[0028] Figure 4 The state of the solidified product 6# of the plugging agent prepared in Example 6 after being dissolved in the dissolving agent GY-1 for 24 hours is shown. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with examples, but the examples of the present invention are only exemplary descriptions, and the implementation methods do not constitute limitations of the present invention under any circumstances.
[0030] Dicyandiamide (DCD), dimethylimidazole (GC), dimethylacetamide (DMA), and dimethylformamide (DMF) were purchased from Chengdu Kelong Chemical Co., Ltd. with analytical grade.
[0031] Thermosetting resin E44 with an epoxy value of 0.44 and thermosetting resin E12 with an epoxy value of 0.12 were purchased from Nantong Xingchen Synthetic Materials Co., Ltd.
[0032] KH550 was purchased from Dongguan Shanyi Plastic Chemical Co., Ltd.
[0033] Calcium carbonate and glass fiber were purchased from Guangdong Bohao Composite Materials Co., Ltd.
[0034] Sodium chloride, calcium chloride and magnesium chloride hexahydrate were all of analytical grade and purchased from Chengdu Kelong Chemicals Co., Ltd.
[0035] Example 1
[0036] The calcium carbonate used in this embodiment is 800 mesh; the average length of the glass fiber is 0.2 mm, and the average diameter is 0.4 mm.
[0037] The preparation method of the controllable self-consolidating plugging agent is as follows:
[0038] Step 1: Weigh 2.136 g DCD and 0.0712 g GC into a stoppered graduated glass test tube;
[0039] Step 2: Weigh 7.12 g of DMA, pour it into a glass graduated test tube containing DCD and GC, and stir it thoroughly at room temperature to completely dissolve DCD and GC to obtain a first mixed solution;
[0040] Step 3: Weigh 35.6 g of heated thermosetting resin E44 (poor fluidity at room temperature), add it to the first mixed solution, and stir well to obtain a second mixed solution;
[0041] Step 4: Weigh 0.088 g of KH550, add it to the second mixed solution, and stir thoroughly to obtain a third mixed solution;
[0042] Step 5: Weigh 3.2 g of calcium carbonate and 1.2 g of glass fiber in sequence, add them into the third mixed solution, stir well, and obtain a self-consolidating plugging agent.
[0043] Place the graduated glass test tube containing the self-consolidating plugging agent in an aging tank and pressurize it to 2MPa, place it in an oven, and heat and cure it at 150°C for 2.5 hours; turn off the oven, do not take out the graduated glass test tube, and slowly cool it naturally in the oven to room temperature and take it out to obtain the consolidated product 1#.
[0044] Example 2
[0045] The calcium carbonate used in this embodiment is 1000 mesh, the average length of the glass fiber is 0.6 mm, and the average diameter is 0.35 mm.
[0046] The preparation method of the controllable self-consolidating plugging agent is as follows:
[0047] Step 1: Weigh 2.880 g DCD and 0.144 g GC into a stoppered graduated glass test tube;
[0048] Step 2: Weigh 7.20 g of DMF, pour it into a glass graduated test tube containing DCD and GC, and stir it thoroughly at room temperature to completely dissolve DCD and GC to obtain a first mixed solution;
[0049] Step 3: Weigh 36 g of heated thermosetting resin E44 (poor fluidity at room temperature), add it to the first mixed solution, and stir well to obtain a second mixed solution;
[0050] Step 4: Weigh 0.12 g of KH550, add it to the second mixed solution, and stir thoroughly to obtain a third mixed solution;
[0051] Step 5: Weigh 2.8 g of calcium carbonate and 1.2 g of glass fiber in sequence, add them into the third mixed solution, stir well, and obtain a self-consolidating plugging agent.
[0052] Place the graduated glass test tube containing the self-consolidating plugging agent in an aging tank and pressurize it to 3MPa, place it in an oven, and heat and cure it at 150°C for 2.2 hours; turn off the oven, do not take out the graduated glass test tube, and slowly cool it naturally in the oven to room temperature and take it out to obtain the consolidated product 2#.
[0053] Example 3
[0054] The calcium carbonate used in this embodiment is 1200 mesh, the average length of the glass fiber is 0.4 mm, and the average diameter is 0.5 mm.
[0055] The preparation method of the controllable self-consolidating plugging agent is as follows:
[0056] Step 1: Weigh 3.640 g DCD and 0.218 g GC into a stoppered graduated glass test tube;
[0057] Step 2: Weigh 8.008 g of DMA, pour it into a glass graduated test tube containing DCD and GC, and stir it thoroughly at room temperature to completely dissolve DCD and GC to obtain a first mixed solution;
[0058] Step 3: Weigh 36.4 g of heated thermosetting resin E44 (poor fluidity at room temperature), add it to the first mixed solution, and stir well to obtain a second mixed solution;
[0059] Step 4: Weigh 0.144 g of KH550, add it to the second mixed solution, and stir thoroughly to obtain a third mixed solution;
[0060] Step 5: Weigh 2.4 g of calcium carbonate and 1.2 g of glass fiber in sequence, add them into the third mixed solution, stir well, and obtain a self-consolidating plugging agent.
[0061] Place the graduated glass test tube containing the self-consolidating plugging agent in an aging tank and pressurize it to 3MPa, place it in an oven, and heat and cure it at 150°C for 2h; turn off the oven, do not take out the graduated glass test tube, and slowly cool it naturally in the oven to room temperature before taking it out to obtain the consolidated product 3#.
[0062] Example 4
[0063] The calcium carbonate used in this embodiment is 1000 mesh, the average length of the glass fiber is 0.3 mm, and the average diameter is 0.45 mm.
[0064] The preparation method of the controllable self-consolidating plugging agent is as follows:
[0065] Step 1: Weigh 2.208 g DCD and 0.074 g GC into a stoppered graduated glass test tube;
[0066] Step 2: Weigh 8.096 g of DMF, pour it into a glass graduated test tube containing DCD and GC, and stir it thoroughly at room temperature to completely dissolve DCD and GC to obtain a first mixed solution;
[0067] Step 3: Weigh 36.8 g of heated thermosetting resin E44 (poor fluidity at room temperature), add it to the first mixed solution, and stir well to obtain a second mixed solution;
[0068] Step 4: Weigh 0.064 g of KH550, add it to the second mixed solution, and stir thoroughly to obtain a third mixed solution;
[0069] Step 5: Weigh 2.0 g of calcium carbonate and 1.2 g of glass fiber in sequence, add them into the third mixed solution, stir well, and obtain a self-consolidating plugging agent.
[0070] The graduated glass test tube containing the self-consolidating plugging agent was placed in an aging tank and pressurized to 2 MPa, placed in an oven, and heated at 150°C for a curing reaction for 1.9 hours; the oven was closed, and the graduated glass test tube was not taken out, and it was slowly cooled naturally in the oven to room temperature and taken out to obtain the solidified product 4#.
[0071] Example 5
[0072] The calcium carbonate used in this embodiment is 1200 mesh, the average length of the glass fiber is 0.5 mm, and the average diameter is 0.6 mm.
[0073] The preparation method of the controllable self-consolidating plugging agent is as follows:
[0074] Step 1: Weigh 3.008 g DCD and 0.150 g GC into a stoppered graduated glass test tube;
[0075] Step 2: Weigh 9.024 g of DMF, pour it into a glass graduated test tube containing DCD and GC, and stir it thoroughly at room temperature to completely dissolve DCD and GC to obtain a first mixed solution;
[0076] Step 3: Weigh 37.6 g of heated thermosetting resin E44 (poor fluidity at room temperature), add it to the first mixed solution, and stir well to obtain a second mixed solution;
[0077] Step 4: Weigh 0.072 g of KH550, add it to the second mixed solution, and stir thoroughly to obtain a third mixed solution;
[0078] Step 5: Weigh 1.6 g of calcium carbonate and 0.8 g of glass fiber in sequence, add them into the third mixed solution, stir well, and obtain a self-consolidating plugging agent.
[0079] The graduated glass test tube containing the self-consolidating plugging agent was placed in an aging tank and pressurized to 3 MPa, placed in an oven, and heated at 150°C for a curing reaction for 1.7 hours; the oven was closed, and the graduated glass test tube was not taken out, and it was slowly cooled naturally in the oven to room temperature and taken out to obtain the solidified product 5#.
[0080] Example 6
[0081] The calcium carbonate used in this embodiment is 800 mesh, the average length of the glass fiber is 0.2 mm, and the average diameter is 0.45 mm.
[0082] The preparation method of the controllable self-consolidating plugging agent is as follows:
[0083] Step 1: Weigh 3.8 g DCD and 0.228 g GC into a stoppered graduated glass test tube;
[0084] Step 2: Weigh 9.5 g of DMA, pour it into a glass graduated test tube containing DCD and GC, and stir it thoroughly at room temperature to completely dissolve DCD and GC to obtain a first mixed solution;
[0085] Step 3: Weigh 38.0 g of heated thermosetting resin E44 (poor fluidity at room temperature), add it to the first mixed solution, and stir well to obtain a second mixed solution;
[0086] Step 4: Weigh 0.08 g of KH550, add it to the second mixed solution, and stir thoroughly to obtain a third mixed solution;
[0087] Step 5: Weigh 1.6 g of calcium carbonate and 0.4 g of glass fiber in sequence, add them into the third mixed solution, stir well, and obtain a self-consolidating plugging agent.
[0088] Place the graduated glass test tube containing the self-consolidating plugging agent in an aging tank and pressurize it to 3MPa, place it in an oven, and heat and cure it at 150°C for 1.2 hours; turn off the oven, do not take out the graduated glass test tube, and slowly cool it naturally in the oven to room temperature and take it out to obtain the consolidated product 6#.
[0089] Comparative Example 1
[0090] The glass fibers used in this embodiment have an average length of 0.2 mm and an average diameter of 0.45 mm.
[0091] The preparation method of the plugging agent is as follows:
[0092] Step 1: Weigh 3.8 g DCD and 0.228 g GC into a stoppered graduated glass test tube;
[0093] Step 2: Weigh 9.5 g of DMA, pour it into a glass graduated test tube containing DCD and GC, and stir it thoroughly at room temperature to completely dissolve DCD and GC to obtain a first mixed solution;
[0094] Step 3: Weigh 38.0 g of heated thermosetting resin E44 (poor fluidity at room temperature), add it to the first mixed solution, and stir well to obtain a second mixed solution;
[0095] Step 4: Weigh 0.08 g KH550, add it to the second mixed solution, and stir thoroughly to obtain a third mixed solution;
[0096] Step 5: Weigh 2.0 g of glass fiber and add it to the third mixed liquid, stir it thoroughly to obtain a plugging agent.
[0097] The graduated glass test tube containing the plugging agent was placed in an aging tank and pressurized to 3 MPa, then placed in an oven and heated at 150°C for a curing reaction for 1.2 hours. The oven was closed, and the graduated glass test tube was not removed. The tube was slowly cooled naturally in the oven to room temperature and then removed to obtain the solidified product D1#.
[0098] Comparative Example 2
[0099] The calcium carbonate used in this embodiment is 800 mesh.
[0100] The preparation method of the plugging agent is as follows:
[0101] Step 1: Weigh 3.8 g DCD and 0.228 g GC into a stoppered graduated glass test tube;
[0102] Step 2: Weigh 9.5 g of DMA and pour it into a glass graduated test tube containing DCD and GC, and stir thoroughly at room temperature to completely dissolve DCD and GC to obtain a first mixed solution;
[0103] Step 3: Weigh 38.0 g of heated thermosetting resin E44 (poor fluidity at room temperature), add it to the first mixed solution, and stir well to obtain a second mixed solution;
[0104] Step 4: Weigh 0.08 g KH550, add it to the second mixed solution, and stir thoroughly to obtain a third mixed solution;
[0105] Step 5: Weigh 2.0 g of calcium carbonate and add it to the third mixed solution, stir it thoroughly to obtain a plugging agent;
[0106] Place the graduated glass test tube containing the plugging agent in an aging tank and pressurize it to 3 MPa, place it in an oven, and heat and cure it at 150°C for 1.2 hours; turn off the oven, do not take out the graduated glass test tube, and slowly cool it naturally in the oven to room temperature and take it out to obtain the solidified product D2#.
[0107] Comparative Example 3
[0108] The calcium carbonate used in this embodiment is 800 mesh, the average length of the glass fiber is 0.2 mm, and the average diameter is 0.45 mm.
[0109] The preparation method of the plugging agent is as follows:
[0110] Step 1: Weigh 3.8 g DCD and 0.228 g GC into a stoppered graduated glass test tube;
[0111] Step 2: Weigh 9.5 g of DMA, pour it into a glass graduated test tube containing DCD and GC, and stir it thoroughly at room temperature to completely dissolve DCD and GC to obtain a first mixed solution;
[0112] Step 3: Weigh 38.0 g of heated thermosetting resin E44 (poor fluidity at room temperature), add it to the first mixed solution, and stir well to obtain a second mixed solution;
[0113] Step 4: Weigh 1.6 g of calcium carbonate and 0.4 g of glass fiber in sequence, add them into the second mixed liquid, stir well, and obtain a plugging agent.
[0114] Place the graduated glass test tube containing the plugging agent in an aging tank and pressurize it to 3 MPa, place it in an oven, and heat and cure it at 150°C for 1.2 hours; turn off the oven, do not take out the graduated glass test tube, and slowly cool it naturally in the oven to room temperature and take it out to obtain the solidified product D3#.
[0115] Comparative Example 4
[0116] The calcium carbonate used in this embodiment is 800 mesh, the average length of the glass fiber is 0.2 mm, and the average diameter is 0.45 mm.
[0117] The preparation method of the plugging agent is as follows:
[0118] Step 1: Weigh 3.8 g of curing agent 593 and 0.228 g of triethanolamine in turn and place them in a stoppered graduated glass test tube;
[0119] Step 2: Weigh 9.5 g of DMA, pour into a glass graduated test tube containing curing agent 593 and triethanolamine, and stir thoroughly to completely dissolve the curing agent 593 and triethanolamine to obtain a first mixed solution;
[0120] Step 3: Weigh 38.0 g of heated thermosetting resin E12 (poor fluidity at room temperature), add it to the first mixed solution, and stir well to obtain a second mixed solution;
[0121] Step 4: Weigh 0.08 g of KH550, add it to the second mixed solution, and stir thoroughly to obtain a third mixed solution;
[0122] Step 5: Weigh 1.6 g of calcium carbonate and 0.4 g of glass fiber in sequence, add them into the third mixed solution, stir well, and obtain a plugging agent.
[0123] The graduated glass test tube containing the plugging agent was placed in an aging tank and pressurized to 3 MPa, then placed in an oven and heated at 150°C for a curing reaction for 1.2 hours. The oven was closed, and the graduated glass test tube was not removed. The tube was slowly cooled naturally in the oven to room temperature and then removed to obtain the solidified product D4#.
[0124] Performance Testing
[0125] Water-based drilling fluid formula: 300mL tap water, 10.5g bentonite N V -1 (purchased from Bohai Drilling Engineering Company), 12g sodium carbonate (purchased from Chengdu Chuanfeng Chemical Co., Ltd.), 1.8g coating agent KPAM (purchased from Chengdu Chuanfeng Chemical Co., Ltd.), 3g filtrate reducer PAC-LV (purchased from Chengdu Chuanfeng Chemical Co., Ltd.), 12g filtrate reducer SMP-2 (purchased from Chengdu Chuanfeng Chemical Co., Ltd.), 12g filtrate reducer SMC (purchased from Chengdu Chuanfeng Chemical Co., Ltd.), 9g anti-collapse agent FT-1 (purchased from Chengdu Chuanfeng Chemical Co., Ltd.), 12g lubricant RH220 (purchased from Chengdu Chuanfeng Chemical Co., Ltd.).
[0126] 1. Determination of rheological properties, temperature resistance and pollution resistance of plugging agents
[0127] Formula for simulated formation water: add 262.5 g of sodium chloride, 22.5 g of calcium chloride and 15 g of magnesium chloride hexahydrate to 300 mL of tap water, so that the mass ratio of sodium chloride: calcium chloride: magnesium chloride hexahydrate is 7:0.6:0.4.
[0128] (1) The plugging agents prepared in the examples and comparative examples were placed at room temperature for different periods of time to investigate the flow of the plugging agents at room temperature before curing. The results are shown in Table 1.
[0129] (2) The plugging agents prepared in the embodiments and comparative examples were placed in an oven at 150° C. for different periods of time to examine the high temperature resistance of the plugging agents after curing. The results are shown in Table 1.
[0130] (3) 100 g of the solidified plugging agent prepared in each embodiment and comparative example was placed in 350 mL of water-based drilling fluid or simulated formation water, and placed in an oven at 150° C. for reaction for 24 h to examine the anti-pollution performance of the plugging agent. The results are shown in Table 1.
[0131] The results are shown in Table 1.
[0132] Table 1 Evaluation of rheological properties, temperature resistance and pollution resistance of plugging agents
[0133]
[0134] According to the results in Table 1, the plugging agent before curing does not gel at room temperature for a long time and has good fluidity, ensuring good pumpability before entering the well; the plugging agent does not melt after 72 hours under high temperature conditions of 150°C, and the plugging agent structure is still intact with good temperature resistance; at the same time, the plugging agent is placed in water-based drilling fluid and simulated formation water and reacted in an oven at 150°C for 24 hours. The plugging agent does not dissolve, does not deform, has a complete structure, and has good anti-pollution performance.
[0135] 2. Determination of compressive strength, pressure-bearing plugging and drillability of plugging agents
[0136] (1) The plugging agents prepared in the embodiments and comparative examples of the present invention were cut into cylindrical specimens with a diameter of 23 mm and a height of 50 mm in accordance with the requirements of GB / T 2567-2008 "Performance Test of Resin Castings". The compressive strength mechanical properties of the products after the plugging agents were solidified were tested using the American MTS rock stress tester.
[0137] (2) Artificial drilling was performed on the natural core to create cracks with a width of about 1 cm. The core with a 1 cm hole was then placed in a beaker with vacuum silicone grease applied to the bottom. The plugging agents prepared in the embodiments and comparative examples were respectively added dropwise to the circular holes of the core until they were filled. The beaker was then placed in an oven and heated to 130° C. for 1.5 h, then heated to 150° C. for 2 h, and then cooled to room temperature after complete curing to obtain a pressure-bearing plugging test core.
[0138] After the pressure plugging test core is placed in the fracture plugging device, the water-based drilling fluid filtrate that has passed through the filter loss meter is injected until fluid flows out from the core outlet or the injection pressure begins to drop. The injection pressure at this time is the breakthrough pressure (plugging pressure).
[0139] (3) The drillability of the plugging agent was tested by a micro-drilling test method. During the test, the plugging agent obtained in each embodiment and comparative example was solidified and cut into a size of 3.8 cm in diameter and 2 cm in length, and then two PDC drill bits were used to simulate the drilling pressure, torque, drill speed and other parameters during formation drilling (blade back angle 20°, side rotation angle 15°, blade thickness 4.5 mm, drill bit outer diameter 32 mm). During the test, 1 mm was pre-drilled first, and then the time taken to drill 3 mm was recorded (wherein, it can be converted into footage, such as m / d or m / h, which is not converted here).
[0140] The drillability grading value of the plugging agent is determined according to the micro-drilling speed. Grades one to four are called "soft rock"; grades five to seven are called "medium-hard rock"; and grades eight to ten are called "hard rock", see Table 2.
[0141] The test results are shown in Table 3.
[0142] According to the results in Table 3, the plugging agents prepared in each embodiment have high compressive strength, all greater than 40MPa; good pressure-bearing plugging performance, and the breakthrough pressure gradient is greater than 85MPa / m; the drillability belongs to level 5 to level 6, and the drillability is good. However, the plugging agents prepared in Comparative Examples 1 to 3 have relatively low strength due to uneven structure, and the plugging effect is not ideal; the plugging agent prepared in Comparative Example 4 has poor strength and cannot meet the needs of malignant leakage treatment.
[0143] Table 2 Rock drillability classification standards
[0144]
[0145] Table 3 Determination of compressive strength, pressure-bearing plugging and drillability of plugging agents
[0146]
[0147] 3. Determination of solubility of plugging agent
[0148] (1) 10 g of the solidified product obtained in each embodiment and comparative example was cut and placed in an aging tank, and 100 mL of an environmentally friendly dissolving agent GY-1 (purchased from Dongguan Jiequan Technology Co., Ltd.) was added;
[0149] (2) The aging tank was pressurized to 1 MPa and placed in an oven at 150°C for dissolution reaction for 2 h, 4 h, 8 h, 18 h and 24 h;
[0150] (3) After the reaction, take out the undissolved plugging agent, place it in a 105°C oven to a constant weight, weigh it, and record the mass of the undissolved plugging agent at different times;
[0151] (4) Calculate the dissolution rate of the plugging agent: dissolution rate = (initial plugging agent mass - remaining undissolved plugging agent mass) / initial plugging agent mass × 100. The results are shown in Table 4.
[0152] in, Figure 1 The solidified product 6# of the plugging agent prepared in Example 6 is shown; Figure 2 The state of the solidified product 6# of the plugging agent prepared in Example 6 after being dissolved in the dissolving agent GY-1 for 2 hours is shown; Figure 3 The state of the solidified product 6# of the plugging agent prepared in Example 6 after being dissolved in the dissolving agent GY-1 for 8 hours is shown; Figure 4 The state of the solidified product 6# of the plugging agent prepared in Example 6 after being dissolved in the dissolving agent GY-1 for 24 hours is shown.
[0153] Table 4 Determination of solubility of plugging agent
[0154]
[0155] According to the results in Table 4, the plugging agents prepared in the embodiments of the present invention have a fast dissolution rate. After 2 hours of dissolution, the structure is obviously destroyed and peeled into blocks. After 8 hours of dissolution, the blocks are further dissolved and gradually become smaller, forming extremely small particles. After 24 hours, the dissolution rate is greater than 90%, which meets the technical requirements of being soluble and easy to unblock after the later plugging construction.
[0156] Although the present invention has been described with reference to specific embodiments, it will be appreciated by those skilled in the art that various changes may be made without departing from the true spirit and scope of the present invention. In addition, the subject matter, spirit and scope of the present invention may be varied to accommodate specific situations, materials, material combinations and methods. All of these changes are included within the scope of the claims of the present invention.
Claims
1. A self-consolidating plugging agent, comprising a thermosetting resin, an inorganic composite material, a silane coupling agent, dicyandiamide, dimethylimidazole and an amide compound.
2. The self-consolidating plugging agent according to claim 1, characterized in that: The epoxy value of the thermosetting resin is above 0.44; Preferably, the thermosetting resin is thermosetting resin E44.
3. The self-consolidating plugging agent according to claim 1, characterized in that: The inorganic composite material is calcium carbonate and glass fiber; Preferably, the mass ratio of the calcium carbonate to the glass fiber is (5 to 8):
3.
4. The self-consolidating plugging agent according to claim 3, characterized in that: The particle size of the calcium carbonate is 800 to 1200 meshes; the length of the glass fiber is 0.2 to 0.6 mm.
5. The self-consolidating plugging agent according to claim 1, characterized in that: The silane coupling agent is silane coupling agent KH550.
6. The self-consolidating plugging agent according to claim 1, characterized in that: The amide compound is dimethylacetamide and / or dimethylformamide.
7. The self-consolidating plugging agent according to claim 1, characterized in that: The mass ratio of the thermosetting resin to the inorganic composite material is (8.1 to 19):1; and / or The mass ratio of the thermosetting resin to the amide compound is (4 to 5):1; and / or The mass ratio of the thermosetting resin, the dicyandiamide and the dimethylimidazole is 100:(6 to 10):(0.2 to 0.6).
8. The self-consolidating plugging agent according to claim 1, characterized in that: Taking the total mass of the inorganic composite material as 100%, the mass of the silane coupling agent is 2% to 4% of the inorganic composite material.
9. A method for preparing the self-consolidating plugging agent according to any one of claims 1 to 8, comprising the following steps: 1) dissolving dicyandiamide and dimethylimidazole in an amide compound to obtain a first mixed solution; 2) adding a thermosetting resin into the first mixed solution and mixing them evenly to obtain a second mixed solution; 3) adding a silane coupling agent to the second mixed solution and mixing them evenly to obtain a third mixed solution; 4) adding the inorganic composite material to the third mixed liquid and mixing them evenly to obtain the self-consolidating plugging agent.
10. Use of the self-consolidating plugging agent according to any one of claims 1 to 8 in plugging leaks in oil and gas drilling.
Citation Information
Patent Citations
Composite gluing material for quick leaking stoppage of pipelines
CN102382607A
Epoxy resin composition and method for preparing adhesive by using same
CN103540103A
Inorganic polymer grouting plugging material and production process thereof
CN112194975A
Epoxy resin glue solution, preparation method thereof, prepreg containing epoxy resin glue solution, preparation method of prepreg, glass fiber epoxy resin copper-clad plate and preparation method of copper-clad plate
CN113831684A
Composite plugging agent as well as preparation method and application thereof
CN114479793A