Preparation method of temperature-sensitive temporary plugging material
By using materials such as cellulose ether, nanosilica and tetrasodium hydroxyethylbenzidine in the dissecting agent, a temperature-sensitive temporary plugging material that can be glued and reversibly changed under high temperature and high mineralization conditions was prepared. , solve the problem of insufficient durability and reversibility in the prior art, and achieve effective temporary blocking and retardation effects in complex oil reservoirs.
Patent Information
- Application Number
- CN202411125598.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-16
AI Technical Summary
The existing distributors are not durable under high temperature and high mineralization conditions, and cannot achieve reversible crosslinking and flexible and viscoelastic characteristics, and cannot meet the needs of complex reservoir development.
Temperature-sensitive temporary plugging materials composed of cellulose ether, nano-silica or sodium soil, tetrasodium hydroxyethylbenziphosphonate, etc. are prepared by adjusting the concentration of enhancer and organic regulator to prepare a temperature-sensitive temporary plugging material that can be between 50 and 100. A temperature-sensitive temporary plugging material that is glued and adjustable at °C can be used to achieve phase transition using temperature changes to achieve sealing and retarding effects.
It realizes high sealing strength and reversible cross-linking under high temperature and high mineralization conditions, adapts to different formation temperatures and mineralization degrees, ensures the glue-forming strength and viscoelasticity of temperature-sensitive temporary plugging materials, and can effectively temporarily plug them. And remove the pores of the formation.
Smart Images

Figure CN119020007A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of profile control, and in particular to a method for preparing a temperature-sensitive temporary plugging material. Background Art
[0002] As oil fields began to enter the high water content development stage in the 1990s, profile control and water plugging technology also reached its peak. In the 21st century, the high water content problem has become one of the problems that oil fields need to solve urgently. Long-term water injection development has further aggravated the heterogeneity of the reservoir, making large pores and high permeability channels in the oil layer common, causing the injected water to flow directly to the bottom of the oil well, seriously reducing the effect of water injection development. Since conventional profile control and water plugging technologies can no longer meet the needs of water injection development, the development of profile control and water plugging technology has entered a new application stage. Among them, the cross-linked gel-type displacement system is not suitable for large-pore and fractured oil reservoirs due to its harsh gelation conditions and low blockage degree. It is not resistant to high temperatures, and the mineralization degree of salt resistance must not exceed 50,000 mg / L. The cross-linking time is slow. The long-term migration of the cross-linked system in the pores of the formation causes diffusion, dilution, shearing, degradation, etc., which makes the cross-linked system, which has harsh gelation conditions on the ground, gel even worse underground, and even makes some cross-linked systems unable to cross-link; pre-cross-linked gel particles: to a certain extent, it is easy to form surface blockage, and has certain requirements for construction technology. In addition, the particles also have certain restrictions on the permeability; foam deep profile control agent: short effective period and complex construction technology.
[0003] Temperature-sensitive temporary plugging materials refer to a type of gel whose phase transition is caused by changes in the gel structure under the influence of temperature. The important feature of temperature-responsive polymers is that they have a critical temperature for phase separation, that is, the polymer solution is a single phase below a certain temperature, and phase separation begins to occur above this temperature. In this case, the polymer has a lower critical solution temperature (LCST), and vice versa, it has an upper critical solution temperature (UCST). Below its critical temperature, the blockage can be released, achieving the effect of temporarily plugging the oil well. Thermosensitive hydrogels with a low critical solution temperature can be roughly divided into two categories, including biomass-based natural polymer thermosensitive gels and synthetic polymer thermosensitive gels. Bio-based natural polymer thermosensitive materials are mainly polysaccharides, cellulose, etc. Synthetic polymer thermosensitive materials include poly (N-isopropylacrylamide) and the like.
[0004] At present, there have been many achievements in the research and invention of profile control agents, but the functions and effects of various products are different. For example, patent CN112480887B discloses a cellulose-based temperature-sensitive gel plugging agent, which is prepared from cellulose, non-ionic monomers, acrylamide, cationic monomers, acryloyloxyethyl trimethyl ammonium chloride, toughening crosslinking agent, and initiator. The provided temperature-sensitive gel plugging agent can change its own phase characteristics as the formation temperature field changes. It is an easy-flowing liquid before being injected into the formation. After being injected into the formation, it undergoes cross-linking and turns into a solid plugging agent with strong adhesion and elastic characteristics, achieving effective plugging of the leakage channel, and has a high pressure resistance to prevent repeated leakage in the formation, and the cross-linking effect is reversible; Patent CN105504158A discloses a smart gel particle that can be re-cross-linked under formation conditions and its preparation method and application, and the smart gel particle is prepared by acrylamide, anionic monomer, cationic monomer, N, N-vinylpyrrolidone, pH value regulator, initiator, cross-linking agent I, cross-linking agent II, stabilizer, nanoparticle material and water. After entering the formation, the smart gel particle can be cross-linked again to form an integrated gel, which can be used in oil field profile control and water plugging, filtration control and / or drilling and completion plugging operations. Patent CN115612237A relates to the field of hydrogel technology, and more specifically, to a preparation method and product of a temperature-sensitive hydrogel. The thermosensitive hydrogel uses acrylic acid and poly-N-isopropylacrylamide as an initiator to polymerize to obtain a polymer material; the polymer material is then coated while hot, cooled, and formed to obtain a thermosensitive hydrogel. The above preparation method increases the temperature at which the volume mutation of the thermosensitive hydrogel occurs from 32°C to 38°C. The thermosensitive hydrogel has water absorption properties, mimics the biological sweating principle, and utilizes the thermosensitive hydrogel's own characteristics that the temperature at which the volume mutation occurs is 38°C. When the ambient temperature is above the temperature at which the volume mutation occurs, the thermosensitive hydrogel slowly releases water molecules to the outside, taking away heat to achieve a cooling effect; when the ambient temperature is below the temperature at which the volume mutation occurs, the thermosensitive hydrogel absorbs air water molecules and returns to its original state.
[0005] Most of the current profile control agents form irreversible chemical cross-linked gels under certain conditions. First, there are deficiencies in achieving temperature control; second, they do not have the reversible cross-linking effect of phase recovery after cooling; third, they do not have certain flexibility and viscoelasticity. Summary of the invention
[0006] Therefore, the present invention provides a method for preparing a temperature-sensitive temporary plugging material. The temperature-sensitive temporary plugging material can achieve a high temperature resistance, high mineralization, and high plugging strength adjustment and displacement agent that meets the conditions of complex oil reservoir development by changing the concentration of the enhancer and the regulator, so as to solve the above technical problems.
[0007] In order to achieve the above object, the present invention adopts the following technical scheme: a method for preparing a temperature-sensitive temporary plugging material, comprising the following raw materials in parts by weight: 100 parts of simulated formation water, 0.5-1 part of cellulose ether, 0.2-0.5 part of a reinforcing agent, and 0.5-1.5 parts of an organic regulator;
[0008] The temperature-sensitive temporary plugging material solution is prepared by the following method:
[0009] (1) Divide 100 portions of simulated formation water into three portions: 60 portions, 20 portions, and 20 portions respectively;
[0010] (2) dissolving cellulose ether in 60 parts of simulated formation water, stirring at 70° C. and 400 rpm for 10 to 20 minutes to obtain a cellulose ether solution;
[0011] (3) The cellulose ether solution stirred in step (2) is placed in ice water and stirred at 400 rpm for 30 to 40 minutes to obtain a main agent solution of a prepared temperature-sensitive plugging agent.
[0012] (4) dissolving the enhancer powder in 20 parts of simulated formation water, stirring with a magnetic stirrer at room temperature for 5 to 10 minutes to form an enhancer aqueous solution;
[0013] (5) dissolving the organic conditioning agent powder in 20 parts of simulated formation water, stirring with a magnetic stirrer at room temperature for 5 to 10 minutes to form an organic conditioning agent aqueous solution;
[0014] (6) The main agent solution, the enhancer aqueous solution and the organic regulator aqueous solution prepared in steps (3) to (5) are dissolved together, and stirred with a magnetic stirrer at room temperature for 5 to 10 minutes to obtain a temperature-sensitive temporary plugging material aqueous solution.
[0015] Preferably, the simulated formation water is of the water type of CaCl2, K + / Na + The concentration is 4000mg / L, Ca 2+ The concentration is 500mg / L, Mg 2+ The concentration is 1000mg / L, Cl - Concentration is 9000mg / L, SO4 2 -Concentration of 250mg / L, HCO3 - The concentration is 250 mg / L and the total mineralization is 15000 mg / L.
[0016] Preferably, the cellulose ether is one of hydroxypropyl methyl cellulose ether and carboxymethyl cellulose ether. The cellulose ether needs to have good solubility, low initial viscosity, high gelling strength and stable gelling. The cellulose ether is selected from hydroxypropyl methyl cellulose ether. Since carboxymethyl cellulose ether has poor gelling strength at a certain temperature after dissolution, it is grade B, while hydroxypropyl methyl cellulose ether has a low initial viscosity at a concentration of 1% and can pass through a formation with a permeability of 5000×10 -3 μm 2 The gel strength at 80-100℃ is G grade, and hydroxypropyl methylcellulose ether is selected as the main agent of a temperature-sensitive temporary plugging material, but the gel is unstable and the viscoelasticity is weak. Therefore, it is necessary to add an enhancer or an organic regulator to enhance the stability and viscoelasticity.
[0017] Preferably, the reinforcing agent is one of nano-silica or sodium clay, and as a reinforcing agent, it can play a certain role in enhancing gelation. As a reinforcing agent, it can play a certain role in enhancing gelation. There are a large number of silanol groups on the surface of silica, which can interact with the hydroxyl groups on the cellulose ether molecules to form hydrogen bonds, increase the entanglement between cellulose ether molecules, increase the viscosity of the compound solution, and also lead to an increase in the gelation temperature.
[0018] Preferably, the organic regulator is one of tetrasodium hydroxyethylidene diphosphonate, sodium tripolyphosphate or disodium ethylenediaminetetraacetate. The organic regulator has a greater influence on the gelation temperature because its molecular structure is similar to the Ca in the simulated formation water. 2+ 、Na + The complexation was formed by changing the Ca 2+ 、Na + The matching relationship between the concentration of ions and the concentration of organic regulators not only plays a role in regulating the gelation temperature but also improves the gel strength. At the same time, the concentration of organic regulators can be changed according to the different mineralization levels in the simulated water to achieve the effect of high mineralization resistance.
[0019] Preferably, the temperature-sensitive temporary plugging material aqueous solution can gel at 50-100°C, and the gelling temperature is adjustable. By adjusting the concentration of the added reinforcing agent and the organic regulator, the gelling temperature can be adjusted. When the temperature is lower than the LCST temperature of the temperature-sensitive temporary plugging material, the temperature-sensitive temporary plugging material can restore the previous low viscosity state and play a temporary plugging role.
[0020] Preferably, the gelling strength of the temperature-sensitive temporary plugging material after gelling is measured by visual code method.
[0021] Beneficial effects of the present invention:
[0022] The present invention provides a temperature-sensitive temporary plugging material, which can change its own phase characteristics as the formation temperature field changes, thereby achieving the effect of phase change. When the temperature is lower than the LCST temperature, the temperature-sensitive temporary plugging material has a low viscosity and can easily flow into the pores of the formation. When the temperature is raised to the LCST temperature, the temperature-sensitive temporary plugging material will turn into a white gel. When the temperature drops back to the LCST temperature, the temperature-sensitive temporary plugging material returns to its previous low-viscosity state, thereby achieving the effect of unblocking and effectively temporarily plugging the formation.
[0023] The present invention provides a temperature-sensitive temporary plugging material, which is applicable to a formation temperature range of 50-100° C., and the gel phase transition temperature can be adjusted according to different formation temperature conditions.
[0024] The temperature-sensitive temporary plugging material provided by the present invention can adjust the gel strength and viscoelasticity by changing the concentration of cellulose ether, reinforcing agent and organic regulator, and can also adapt to different Ca 2+ 、Na + Concentration of simulated formation water. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the gelling conditions of the temperature-sensitive temporary plugging materials of Example 1, Example 2, Example 3 and Comparative Example 1 of the present invention at 50° C.;
[0026] Figure 2 It is a schematic diagram of the gelling of the temperature-sensitive temporary plugging materials of Comparative Examples 2, 3, 4 and 5 of the present invention at 50°C. DETAILED DESCRIPTION
[0027] In order to further explain the technical solution of the present invention, it is described in detail below through specific embodiments.
[0028] Example 1
[0029] A temperature-sensitive temporary plugging material is composed of the following raw materials in parts by weight: 100 parts of simulated formation water; cellulose ether: 1 part of hydroxypropyl methylcellulose ether; reinforcing agent: 0.2 parts of nano silicon dioxide; and organic regulator: 1 part of tetrasodium hydroxyethylidene diphosphonate.
[0030] A method for preparing a temperature-sensitive temporary plugging material comprises the following steps:
[0031] (1) Divide 100 portions of simulated formation water into three portions: 60 portions, 20 portions, and 20 portions respectively;
[0032] (2) dissolving cellulose ether in 60 parts of simulated formation water, stirring at 70° C. and 400 rpm for 10 to 20 minutes to obtain a cellulose ether solution;
[0033] (3) The cellulose ether solution stirred in step (2) is placed in ice water and stirred at 400 rpm for 30 to 40 minutes to obtain a main agent solution of a prepared temperature-sensitive plugging agent.
[0034] (4) dissolving the enhancer powder in 20 parts of simulated formation water, stirring with a magnetic stirrer at room temperature for 5 to 10 minutes to form an enhancer aqueous solution;
[0035] (5) dissolving the organic conditioning agent powder in 20 parts of simulated formation water, stirring with a magnetic stirrer at room temperature for 5 to 10 minutes to form an organic conditioning agent aqueous solution;
[0036] (6) The main agent solution, the enhancer aqueous solution and the organic regulator aqueous solution prepared in steps (3) to (5) are dissolved together, and stirred with a magnetic stirrer at room temperature for 5 to 10 minutes to obtain a temperature-sensitive temporary plugging material aqueous solution.
[0037] Example 2
[0038] A temperature-sensitive temporary plugging material is composed of the following raw materials in parts by weight: 100 parts of simulated formation water; cellulose ether: 1 part of hydroxypropyl methylcellulose ether; reinforcing agent: 0.5 part of nano silicon dioxide; and organic regulator: 1 part of tetrasodium hydroxyethylidene diphosphonate.
[0039] A method for preparing a temperature-sensitive temporary plugging material comprises the following steps:
[0040] (1) Divide 100 portions of simulated formation water into three portions: 60 portions, 20 portions, and 20 portions respectively;
[0041] (2) dissolving cellulose ether in 60 parts of simulated formation water, stirring at 70° C. and 400 rpm for 10 to 20 minutes to obtain a cellulose ether solution;
[0042] (3) The cellulose ether solution stirred in step (2) is placed in ice water and stirred at 400 rpm for 30 to 40 minutes to obtain a main agent solution of a prepared temperature-sensitive plugging agent.
[0043] (4) dissolving the enhancer powder in 20 parts of simulated formation water, stirring with a magnetic stirrer at room temperature for 5 to 10 minutes to form an enhancer aqueous solution;
[0044] (5) dissolving the organic conditioning agent powder in 20 parts of simulated formation water, stirring with a magnetic stirrer at room temperature for 5 to 10 minutes to form an organic conditioning agent aqueous solution;
[0045] (6) The main agent solution, the enhancer aqueous solution and the organic regulator aqueous solution prepared in steps (3) to (5) are dissolved together, and stirred with a magnetic stirrer at room temperature for 5 to 10 minutes to obtain a temperature-sensitive temporary plugging material aqueous solution.
[0046] Example 3
[0047] A temperature-sensitive temporary plugging material is composed of the following raw materials in parts by weight: 100 parts of simulated formation water; cellulose ether: 1 part of hydroxypropyl methylcellulose ether; reinforcing agent: 0.2 parts of nano silicon dioxide; and organic regulator: 0.5 parts of tetrasodium hydroxyethylidene diphosphonate.
[0048] A method for preparing a temperature-sensitive temporary plugging material comprises the following steps:
[0049] (1) Divide 100 portions of simulated formation water into three portions: 60 portions, 20 portions, and 20 portions respectively;
[0050] (2) dissolving cellulose ether in 60 parts of simulated formation water, stirring at 70° C. and 400 rpm for 10 to 20 minutes to obtain a cellulose ether solution;
[0051] (3) The cellulose ether solution stirred in step (2) is placed in ice water and stirred at 400 rpm for 30 to 40 minutes to obtain a main agent solution of a prepared temperature-sensitive plugging agent.
[0052] (4) dissolving the enhancer powder in 20 parts of simulated formation water, stirring with a magnetic stirrer at room temperature for 5 to 10 minutes to form an enhancer aqueous solution;
[0053] (5) dissolving the organic conditioning agent powder in 20 parts of simulated formation water, stirring with a magnetic stirrer at room temperature for 5 to 10 minutes to form an organic conditioning agent aqueous solution;
[0054] (6) The main agent solution, the enhancer aqueous solution and the organic regulator aqueous solution prepared in steps (3) to (5) are dissolved together, and stirred with a magnetic stirrer at room temperature for 5 to 10 minutes to obtain a temperature-sensitive temporary plugging material aqueous solution.
[0055] Table 1 Materials and amounts used in Examples 1-3
[0056]
[0057] The temperature-sensitive temporary plugging material aqueous solution prepared in the above three embodiments can be gelled at 50-100°C, and the gelling is adjustable, such as Figure 1As shown, by adjusting the concentration of the added reinforcing agent and the organic regulator, the gelling temperature can be adjusted. When the temperature is lower than the LCST temperature of the temperature-sensitive temporary plugging material, the temperature-sensitive temporary plugging material can restore its previous low viscosity state and play a temporary plugging role.
[0058] Comparative Example 1
[0059] A method for preparing a temperature-sensitive temporary plugging material. The difference between this comparative example and Example 1 is that the reinforcing agent is replaced with sodium clay, and the other raw material types, amounts, experimental steps and experimental parameters are consistent with Example 1.
[0060] Comparative Example 2
[0061] A method for preparing a temperature-sensitive temporary plugging material. The difference between this comparative example and Example 1 is that the organic regulator is replaced with sodium tripolyphosphate, and the other raw material types, amounts, experimental steps and experimental parameters are consistent with Example 1.
[0062] Comparative Example 3
[0063] A method for preparing a temperature-sensitive temporary plugging material. The difference between this comparative example and Example 1 is that the organic regulator is replaced with disodium ethylenediaminetetraacetate, and the other raw material types, amounts, experimental steps and experimental parameters are consistent with Example 1.
[0064] Comparative Example 4
[0065] A method for preparing a temperature-sensitive temporary plugging material, the difference between this comparative example and Example 1 is that the concentration of the organic regulator is increased to 1.5%. The other raw material types, dosages, experimental steps and experimental parameters are consistent with Example 1.
[0066] Comparative Example 5
[0067] A method for preparing a temperature-sensitive temporary plugging material. The difference between this comparative example and Example 1 is that: simulated formation water, Ca 2+ The concentration is 500mg / L, Mg 2+ The concentration is 1000 mg / L, the total mineralization is 30000 mg / L, and the other raw material types, dosages, experimental steps and experimental parameters are consistent with those in Example 1.
[0068] Performance testing:
[0069] 1. Observe the gelling strength of the temperature-sensitive temporary plugging material by visual code observation method:
[0070] The temperature-sensitive temporary plugging material provided in the embodiment was dissolved in simulated formation water according to the above steps, and the gel strength of the solution at 50-100°C was measured. The state of the temporary plugging material at different temperatures was observed. The results are shown in Table 1.
[0071] First, based on the gel strength of the thermosensitive gel, the effects of the type and amount of the enhancer, the type and amount of the organic regulator, and the mineralization of the simulated formation water on the gel strength were observed, and the gel strength of Examples 1-3 and Comparative Examples 1-4 were compared. The gel strength was determined by the code method, and the results are shown in Table 2
[0072] Table 2 Code method gel strength
[0073]
[0074] As can be seen from Table 2, by comparing Example 1 and Comparative Example 4, when the reinforcing agent is sodium soil, the gelling effect is the worst at 50-100°C, and the sodium soil has poor solubility and will precipitate, so sodium soil is not considered in this application. After adding the reinforcing agent nano-silica, the overall gelling strength of the temperature-sensitive temporary plugging material becomes higher, indicating that the effect of the reinforcing agent nano-silica is obvious, reaching grade H at 90-100°C.
[0075] As shown in Table 2, by comparing Example 1 with Example 2, it is found that when the concentration of the reinforcing agent nano-silicon dioxide increases, the gel strength decreases instead, which indicates that under the experimental conditions, the concentration of nano-silicon dioxide in Example 1 is appropriate.
[0076] As shown in Table 2, when the concentrations of cellulose ether and reinforcing agent are unchanged, the type of organic regulator is tetrasodium hydroxyethylidene diphosphonate, sodium tripolyphosphate or disodium ethylenediaminetetraacetate. The gel strength of tetrasodium hydroxyethylidene diphosphonate is better than that of the other two organic regulators. The addition of tetrasodium hydroxyethylidene diphosphonate is found to improve the viscoelasticity of the temporary plugging material through rheological tests, so tetrasodium hydroxyethylidene diphosphonate is selected as the organic regulator in the temperature-sensitive temporary plugging material.
[0077] As shown in Table 2, by comparing Example 1, Example 3 and Comparative Example 4, it can be seen that when other conditions remain unchanged, the gelling strength of the entire temporary plugging system in Example 1 is the highest, and the concentration of the organic regulator tetrasodium hydroxyethylidene diphosphonate is more suitable at 1%. However, this solution still cannot meet the gelling requirements between 50 and 60°C.
[0078] As shown in Table 2, by comparing Example 1 with Comparative Example 5, when the overall mineralization of the simulated formation water increases from 15,000 to 30,000 mg / L, the Ca 2+ Mg 2+The ion concentration remains unchanged, and the temporary plugging material can gel at 50-60°C. High concentration of salt can weaken the hydration of cellulose ether macromolecules and promote gelation. At the same time, sodium, calcium and magnesium ions can also react with tetrasodium hydroxyethylidene diphosphonic acid. Tetrasodium hydroxyethylidene diphosphonic acid can not only inhibit the effect of calcium and magnesium on cellulose ether molecules, but also form a new cross-linking network with sodium, calcium and magnesium ions to improve the degree of gelation, satisfying the requirement that the temperature-sensitive temporary plugging material can gel at 50-100°C.
[0079] 2. Gel formation reversibility test
[0080] like Figure 2 As shown, the temperature-sensitive temporary plugging material examples 1-3 and comparative examples 1-5 are placed at their gelation temperature for a certain period of time. After gelation, they are taken out and placed at room temperature for a period of time. It can be seen that examples 1-3 and comparative examples 1-5 can return to the original low-viscosity fluid at room temperature for 30 minutes, indicating that the temperature-sensitive temporary plugging material provided by the present application can plug the formation and then return to the low-viscosity fluid, thereby playing a temporary plugging role.
[0081] The above description is only a preferred example of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a temperature-sensitive temporary plugging material, characterized in that: The method is composed of the following raw materials in parts by weight: 100 parts of simulated formation water, 0.5-1 parts of cellulose ether, 0.2-0.5 parts of reinforcing agent, and 0.5-1.5 parts of organic regulator; The temperature-sensitive temporary plugging material solution is prepared by the following method: (1) Divide 100 portions of simulated formation water into three portions: 60 portions, 20 portions, and 20 portions respectively; (2) dissolving cellulose ether in 60 parts of simulated formation water, stirring at 70° C. and 400 rpm for 10 to 20 minutes to obtain a cellulose ether solution; (3) The cellulose ether solution stirred in step (2) is placed in ice water and stirred at 400 rpm for 30 to 40 minutes to obtain a main agent solution of the prepared temperature-sensitive plugging agent. (4) dissolving the enhancer powder in 20 parts of simulated formation water, stirring with a magnetic stirrer at room temperature for 5 to 10 minutes to form an enhancer aqueous solution; (5) dissolving the organic conditioning agent powder in 20 parts of simulated formation water, stirring with a magnetic stirrer at room temperature for 5 to 10 minutes to form an organic conditioning agent aqueous solution; (6) The main agent solution, the enhancer aqueous solution and the organic regulator aqueous solution prepared in steps (3) to (5) are dissolved together, and stirred with a magnetic stirrer for 5 to 10 minutes at room temperature to obtain a temperature-sensitive temporary plugging material aqueous solution.
2. The method for preparing a temperature-sensitive temporary plugging material according to claim 1, characterized in that: The simulated formation water is of the water type of CaCl2, K + / Na + The concentration is 4000mg / L, Ca 2+ The concentration is 500mg / L, Mg 2+ The concentration is 1000mg / L, Cl - Concentration is 9000mg / L, SO4 2- The concentration is 250mg / L, HCO3 - The concentration is 250 mg / L and the total mineralization is 15000 mg / L.
3. The method for preparing a temperature-sensitive temporary plugging material according to claim 1, characterized in that: The cellulose ether is one of hydroxypropyl methyl cellulose ether and carboxymethyl cellulose ether.
4. The method for preparing a temperature-sensitive temporary plugging material according to claim 1, characterized in that: The reinforcing agent is one of nano silicon dioxide or sodium earth.
5. The method for preparing a temperature-sensitive temporary plugging material according to claim 1, characterized in that: The organic regulator is one of tetrasodium hydroxyethylidene diphosphonate, sodium tripolyphosphate or disodium ethylenediaminetetraacetate.
6. A temperature-sensitive temporary plugging material obtained by the method for preparing a temperature-sensitive temporary plugging material according to any one of claims 1 to 5, characterized in that: The temperature-sensitive temporary plugging material aqueous solution can gel at 50-100° C., and the gelling is adjustable.
7. The method for preparing a temperature-sensitive temporary plugging material according to claim 6, characterized in that: The gelling strength of the temperature-sensitive temporary plugging material after gelling is measured by visual code method.
Citation Information
Patent Citations
Reverse-phase temporary plugging agent and preparation method thereof
CN106634911A
Cellulose-based temperature-sensitive gel plugging agent and preparation method thereof
CN112480887A
Temporary plugging agent for heavy oil well as well as preparation method and application of temporary plugging agent
CN115678522A
Layered water plugging process
CN117345155A