Electrochromic material with respectively adjustable visible light transmittance and near-infrared light transmittance, preparation method of electrochromic material and electrochromic device
By using anode coloring material and high and low potential cathode coloring material in electrochromic devices, independent adjustment of visible light and near infrared light transmittance is achieved, and the problem that the prior art cannot adjust the near infrared light transmittance is solved. , improves the imaging effect of the camera under different light conditions.
Patent Information
- Application Number
- CN202411164680.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-26
AI Technical Summary
Existing electrochromic devices cannot effectively adjust the transmittance of near-infrared light, resulting in the inability to assist in night imaging.
The visible-near-infrared light transmittance is formed by mixing anode coloring material, a high-potential cathode coloring material with an absorption peak in the near-infrared light wavelength range, and a low-potential cathode coloring material with an absorption peak in the visible light wavelength range. Color-changing material, the transmittance of electrochromic devices to visible and near-infrared light is adjusted through redox reactions.
The independent adjustment of visible and near-infrared light transmittance is achieved, and the assisted imaging during the day and at night can be achieved, improving the camera's shooting effect under different light conditions.
Smart Images

Figure BDA0005007504110000021 
Figure BDA0005007504110000022 
Figure BDA0005007504110000023
Abstract
Description
Technical Field
[0001] The invention relates to an electrochromic material with adjustable visible light and near infrared light transmittances, a preparation method thereof and an electrochromic device. Background Art
[0002] At present, electrochromic devices use electrochromic materials to undergo redox reactions under voltage to change the transmittance of the electrochromic materials to light, which in turn changes the color and transparency of the electrochromic devices. For example, a Chinese patent with announcement number CN214669989U discloses an electrochromic device.
[0003] Electrochromic devices are used in cameras mainly to solve the problem of overexposure of the captured image when the external light is too strong. Cameras generally use visible light for imaging in daytime environments. When the visible light is too strong, it is necessary to reduce the transmittance of the electrochromic device to visible light to suppress overexposure of the captured image. When the intensity of visible light is normal, it is necessary to increase the transmittance of the electrochromic device to visible light to prevent the captured image from being too dark. Therefore, the electrochromic device needs to adjust the transmittance of visible light to assist in daytime imaging. Cameras mostly use infrared imaging in nighttime environments. At this time, if the near-infrared light is too strong, it is necessary to reduce the transmittance of the electrochromic device to near-infrared light to suppress overexposure of the captured image. If the intensity of the near-infrared light is normal, it is necessary to increase the transmittance of the electrochromic device to near-infrared light to prevent unclear images. Therefore, the electrochromic device needs to adjust the transmittance of near-infrared light to assist in night imaging.
[0004] However, most existing electrochromic devices can only effectively adjust the transmittance of visible light, but cannot effectively adjust the transmittance of near-infrared light. Therefore, existing electrochromic devices cannot adjust the transmittance of near-infrared light to assist night imaging. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the defects of the prior art and provide an electrochromic material with adjustable visible light and near-infrared light transmittances. The electrochromic device made of the electrochromic material with adjustable visible light and near-infrared light transmittances can adjust and control the transmittance of visible light and the transmittance of near-infrared light respectively, so that the electrochromic device can adjust the transmittance of visible light to assist daytime imaging, and can also adjust the transmittance of near-infrared light to assist nighttime imaging.
[0006] In order to solve the above technical problems, the technical solution of the present invention is: an electrochromic material with adjustable visible light and near-infrared light transmittance, which is mainly composed of an anode color-changing material, a high-potential cathode color-changing material with an absorption peak in the near-infrared light wavelength range, and a low-potential cathode color-changing material with an absorption peak in the visible light wavelength range; wherein the redox potential of the high-potential cathode color-changing material is higher than that of the low-potential cathode color-changing material.
[0007] Furthermore, the molar ratio of the sum of the high potential cathode color-changing material and the low potential cathode color-changing material to the anode color-changing material is 1:1.
[0008] Furthermore, the concentrations of the anode color-changing material, the high-potential cathode color-changing material and the low-potential cathode color-changing material are all 1 to 100 mM.
[0009] A combination of an anodic color-changing material, a high-potential cathode color-changing material and a low-potential cathode color-changing material is further provided, wherein the anodic color-changing material is 1,1':4'1"-terphenyl-4,4"-dithiol, and has the structural formula:
[0010]
[0011] The high potential cathode color-changing material is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate, and the structural formula is:
[0012]
[0013] The low potential cathode color changing material is hexyl viologen bistetrafluoroborate, and the structural formula is:
[0014]
[0015] Further provided is another combination of an anode color-changing material, a high-potential cathode color-changing material and a low-potential cathode color-changing material, wherein the anode color-changing material is 5,10-diisopropyl-5,10-dihydrophenazine, and has the structural formula:
[0016]
[0017] The high potential cathode color-changing material is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate, and the structural formula is:
[0018]
[0019] The low potential cathode color-changing material is 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate), and the structural formula is:
[0020]
[0021] The present invention also provides a method for preparing the electrochromic material with adjustable visible light and near-infrared light transmittances, the method comprising the following steps:
[0022] S1: Take appropriate amounts of anode color-changing material, high-potential cathode color-changing material and low-potential cathode color-changing material and mix them into a solution.
[0023] Furthermore, the method further comprises:
[0024] S0: Prepare anode color-changing materials, high-potential cathode color-changing materials and low-potential cathode color-changing materials.
[0025] Further, when the anode color-changing material is 1,1':4'1"-terphenyl-4,4"-dithiol, the high potential cathode color-changing material is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate, and the low potential cathode color-changing material is hexyl viologen bis-tetrafluoroborate, the specific operation of step S0 is as follows:
[0026] Wherein, the step of preparing the anode color changing material 1,1':4'1"-terphenyl-4,4"-dithiol in step S0 is:
[0027] M1: bromobenzene, phenylboric acid, Pd(OAc)2, potassium carbonate, DMF and water are added to a microwave reaction device and heated by microwave irradiation for reaction. After the reaction is completed, ethyl acetate is used to extract the product 1,1':4',1"-terphenyl from the reaction mixture. A mixture of ethyl acetate and n-hexane in a ratio of 1:1 is then used as an eluent to purify the extracted product 1,1':4',1"-terphenyl by column chromatography;
[0028] M2: Under a nitrogen atmosphere, chlorosulfonic acid and dichloromethane were added to the reaction vessel, and then the 1,1':4',1"-terphenyl obtained in step M1 was added dropwise, the reaction temperature was maintained at 0°C, and then the temperature was raised to room temperature and stirred. After the reaction was completed, a large amount of saturated brine was added to the system, and then the organic phase was extracted with dichloromethane and collected. The organic phase was then dried with MgSO4 and the solvent in the organic phase was removed by rotary evaporation, and then separated by column chromatography to obtain 1,1':4',1"-terphenyl-4,4"-disulfonyl chloride;
[0029] M3: Take the 1,1':4',1"-terphenyl-4,4"-disulfonyl chloride synthesized in step M2 and dissolve it in tetrahydrofuran solvent, add LiAlH4 and reflux reaction, add appropriate amount of ice water to quench after the reaction is completed, then add concentrated hydrochloric acid to adjust the pH value to less than or equal to 1, then filter to remove precipitated impurities, extract the solution with dichloromethane and collect the organic phase, then dry the organic phase with MgSO4 and spin dry the solvent in the organic phase to obtain light yellow crystalline 1,1':4'1"-terphenyl-4,4"-dithiol;
[0030] Wherein, the step of preparing the high potential cathode color-changing material (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate in step S0 is:
[0031] N1: Add dichloroethane, tetra-tert-butylferrocene and 6-bromohexanoyl chloride to a reaction vessel under nitrogen protection, cool the mixed solution in the reaction vessel to 0°C, then put AlCl3 into the reaction vessel, pour the reaction mixture into stirring water and stir after the reaction is completed, then add sufficient ether to form a stratification of the reaction mixture, then add concentrated hydrochloric acid and zinc powder to the system to ensure that the iron salt exists in a divalent form, collect the organic phase and the aqueous phase respectively with a separatory funnel after the reduction is completed, then add ether to the system to continue extraction and continue to collect the organic phase and the aqueous phase with a separatory funnel, then combine all the collected organic phases, wash the organic phase with an aqueous solution containing NaHCO3 and salt, then dry the organic phase with MgSO4, filter the organic phase, and then rotary evaporate to remove the solvent in the organic phase to obtain a red oily substance; add the red oily substance to a vacuum-assisted silica gel column and elute with n-hexane to remove residual ferrocene, and finally rotary evaporate the eluted product to remove the solvent to obtain 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone;
[0032] N2: Dissolve AlCl3 in dry ether and place in a Schlenk flask, cool the solution in the Schlenk flask to 0°C, inject LiAlH4 into the Schlenk flask with a syringe, and then heat the suspension obtained by the reaction to room temperature and stir; take 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone prepared in step N1 and add it to the Schlenk flask, then heat the reaction solution in the Schlenk flask to reflux and then cool to room temperature. After the reaction is completed, add the Schlenk flask to a flask and heat to reflux. nk flask, adding water to quench the reaction solution, then adding ether to extract the reaction solution and separating the organic phase with a separatory funnel, then washing the separated organic phase with an aqueous solution containing NaHCO3 and salt, and then drying with MgSO4, filtering and then removing the solvent in the organic phase by rotary evaporation to obtain a yellow-orange oil; adding the yellow-orange oil to a vacuum-assisted silica gel column and eluting with n-hexane to separate, and the product obtained after elution is separated by rotary evaporation to remove the solvent to obtain 6-bromo-1-(tetra-tert-butylferrocenylhexane);
[0033] N3: triethylamine, acetonitrile and 6-bromo-1-(tetra-tert-butylferrocenehexane) prepared in step N2 are added to a reaction container, the solution in the reaction container is heated to reflux for reaction, the solvent is removed by rotary evaporation after the reaction is cooled to room temperature to obtain a crude product, the crude product is washed with ether, filtered and then dried in a vacuum to obtain a bromide salt, the bromide salt is dissolved in methanol and an excess of NaBF4 aqueous solution is added to react, the methanol is removed by rotary evaporation from the solution obtained by the reaction to obtain an orange precipitate, the orange precipitate is collected on a filter element, repeatedly recrystallized, and stored for standby use; wherein the orange precipitate is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate;
[0034] Wherein, the step of preparing the low potential cathode color-changing material hexyl viologen bistetrafluoroborate in step S0 is:
[0035] Add 4-4'-bipyridine, 1-bromohexane and N,N'-dimethylformamide solvent to the reaction container and heat to reflux to react to obtain a precipitate. After the reaction is completed, cool to room temperature and collect the precipitate by vacuum filtration. Then, wash the collected precipitate with N,N'-dimethylformamide and acetone solvent respectively, and then vacuum dry the precipitate to obtain the product hexyl viologen bistetrafluoroborate.
[0036] Further, when the anode color-changing material is 5,10-diisopropyl-5,10-dihydrophenazine, the high potential cathode color-changing material is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate, and the low potential cathode color-changing material is 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate), the specific operation of step S0 is as follows:
[0037] The step of preparing the anode color-changing material 5,10-diisopropyl-5,10-dihydrophenazine in step S0 is as follows:
[0038] A finely ground metal alloy, phenazine and 1,2-dimethoxyethane in a potassium-sodium ratio of 10:1 are placed in a reaction vessel and stirred until a brick-red slurry is formed, then the stirring is stopped and the reaction is allowed to stand, then 2-bromopropane is added to the reaction mixture and stirred, after the reaction is completed, the precipitate in the reaction mixture is filtered out, and then the solvent in the reaction mixture is removed by rotary evaporation, and then a mixture of hexane and ethyl acetate in a ratio of 8:2 is used as an eluent to elute and separate the reaction mixture through a vacuum-assisted silica gel column to obtain a white solid, and the white solid is dissolved in methanol and recrystallized to obtain 5,10-diisopropyl-5,10-dihydrophenazine;
[0039] Wherein, the step of preparing the high potential cathode color-changing material (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate in step S0 is:
[0040] N1: Add dichloroethane, tetra-tert-butylferrocene and 6-bromohexanoyl chloride to a reaction vessel under nitrogen protection, cool the mixed solution in the reaction vessel to 0°C, then put AlCl3 into the reaction vessel, pour the reaction mixture into stirring water and stir after the reaction is completed, then add sufficient ether to form a stratification of the reaction mixture, then add concentrated hydrochloric acid and zinc powder to the system to ensure that the iron salt exists in a divalent form, collect the organic phase and the aqueous phase respectively with a separatory funnel after the reduction is completed, then add ether to the system to continue extraction and continue to collect the organic phase and the aqueous phase with a separatory funnel, then combine all the collected organic phases, wash the organic phase with an aqueous solution containing NaHCO3 and salt, then dry the organic phase with MgSO4, filter the organic phase, and then rotary evaporate to remove the solvent in the organic phase to obtain a red oily substance; add the red oily substance to a vacuum-assisted silica gel column and elute with n-hexane to remove residual ferrocene, and finally rotary evaporate the eluted product to remove the solvent to obtain 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone;
[0041] N2: Dissolve AlCl3 in dry ether and place in a Schlenk flask, cool the solution in the Schlenk flask to 0°C, inject LiAlH4 into the Schlenk flask with a syringe, and then heat the suspension obtained by the reaction to room temperature and stir; take 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone prepared in step N1 and add it to the Schlenk flask, then heat the reaction solution in the Schlenk flask to reflux and then cool to room temperature. After the reaction is completed, add the Schlenk flask to a flask and heat to reflux. nk flask, adding water to quench the reaction solution, then adding ether to extract the reaction solution and separating the organic phase with a separatory funnel, then washing the separated organic phase with an aqueous solution containing NaHCO3 and salt, and then drying with MgSO4, filtering and then removing the solvent in the organic phase by rotary evaporation to obtain a yellow-orange oil; adding the yellow-orange oil to a vacuum-assisted silica gel column and eluting with n-hexane to separate, and the product obtained after elution is separated by rotary evaporation to remove the solvent to obtain 6-bromo-1-(tetra-tert-butylferrocenylhexane);
[0042] N3: triethylamine, acetonitrile and 6-bromo-1-(tetra-tert-butylferrocenehexane) prepared in step N2 are added to a reaction container, the solution in the reaction container is heated to reflux for reaction, the solvent is removed by rotary evaporation after the reaction is cooled to room temperature to obtain a crude product, the crude product is washed with ether, filtered and then dried in a vacuum to obtain a bromide salt, the bromide salt is dissolved in methanol and an excess of NaBF4 aqueous solution is added to react, the methanol is removed by rotary evaporation from the solution obtained by the reaction to obtain an orange precipitate, the orange precipitate is collected on a filter element, repeatedly recrystallized, and stored for standby use; wherein the orange precipitate is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate;
[0043] The step of preparing the low potential cathode color changing material 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate) in step S0 is:
[0044] 3,5-dimethylaniline is added to a solution of dimethylformamide and water in a ratio of 3:2, and heated under a nitrogen atmosphere for reflux reaction. Then, 1,1'-di(2,4-dinitrophenyl)-4,4'-bipyridine is dissolved in water and added to the reaction solution through a constant pressure dropping funnel for reflux reaction. After the reaction is cooled, the yellow-brown precipitate produced is filtered out, and the water in the filtrate is removed by rotary evaporation to obtain a concentrated solution. Then, a large amount of acetone is added to the concentrated solution for reaction to obtain a yellow precipitate. After filtering and collecting the yellow precipitate, the yellow precipitate is dissolved in a small amount of water and an excess of NaBF4 is added for reaction to obtain an orange precipitate. The obtained orange precipitate is purified by repeated crystallization with methanol to obtain an off-white solid, which is 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate).
[0045] The present invention also provides an electrochromic device, comprising a device body, wherein the device body has an electrochromic layer, and the electrochromic layer comprises any one of the electrochromic materials with adjustable visible light and near-infrared light transmittances as described above.
[0046] After adopting the above technical scheme, in the electrochromic device made of the electrochromic material with adjustable visible light and near-infrared light transmittance according to the embodiment of the present application, the absorption peak of the low-potential cathode color-changing material is located in the visible light wavelength range, so when the applied voltage changes, the low-potential cathode color-changing material will undergo an oxidation-reduction reaction with the anode color-changing material and then be used to adjust the transmittance of visible light. The absorption peak of the high-potential cathode color-changing material is located in the near-infrared light wavelength range, so when the applied voltage changes, the high-potential cathode color-changing material will undergo an oxidation-reduction reaction with the anode color-changing material and then be used to adjust the transmittance of near-infrared light. Therefore, the electrochromic device made of the electrochromic material with adjustable visible light and near-infrared light transmittance according to the embodiment of the present application can adjust and control the transmittance of visible light and the transmittance of near-infrared light respectively. When the electrochromic device is used in a camera, it can adjust the transmittance of visible light to assist daytime imaging, and can adjust the transmittance of near-infrared light to assist night imaging.
[0047] In the electrochromic device made of the electrochromic material with adjustable visible light and near-infrared light transmittance according to the embodiment of the present application, since the redox potential of the high-potential cathode color-changing material is higher than the redox potential of the low-potential cathode color-changing material, in the present embodiment, when the voltage applied to the electrochromic device changes in the low voltage range of 0 to 1.2 V, the low-potential cathode color-changing material will first undergo a redox reaction with the anode color-changing material as the voltage changes, thereby being able to cause a significant change in the transmittance of visible light, that is, being able to have a better regulating effect on the transmittance of visible light, while the transmittance of near-infrared light will not change significantly at this time. When the voltage applied to the electrochromic device changes in the high voltage range of 1.2 to 2V, the high-potential cathode color-changing material will undergo an oxidation-reduction reaction with the anode color-changing material as the voltage changes, thereby causing the transmittance of near-infrared light to change significantly, that is, it can have a better regulating effect on the transmittance of near-infrared light. At this time, the low-potential cathode color-changing material has been reduced to a large extent, so the transmittance of visible light will not change significantly, thereby realizing the separate regulation of the visible light transmittance and the near-infrared light transmittance under different voltages. DETAILED DESCRIPTION
[0048] The present invention provides an electrochromic material with adjustable visible light and near-infrared light transmittance, a preparation method thereof, and an electrochromic device. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the desired effect. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they all fall within the scope of protection of the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications of this article without departing from the content, spirit, and scope of the present invention to realize and apply the technology of the present invention.
[0049] The present invention provides an electrochromic material with adjustable visible light and near-infrared light transmittance, which is mainly formed by mixing an anode color-changing material, a high-potential cathode color-changing material whose absorption peak is in the near-infrared light wavelength range, and a low-potential cathode color-changing material whose absorption peak is in the visible light wavelength range; wherein the redox potential of the high-potential cathode color-changing material is higher than that of the low-potential cathode color-changing material.
[0050] Specifically, in the electrochromic device made of the electrochromic material with adjustable visible light and near-infrared light transmittance according to the embodiment of the present application, the absorption peak of the low-potential cathode color-changing material is located in the visible light wavelength range, so when the applied voltage changes, the low-potential cathode color-changing material will undergo an oxidation-reduction reaction with the anode color-changing material and then be used to adjust the transmittance of visible light. The absorption peak of the high-potential cathode color-changing material is located in the near-infrared light wavelength range, so when the applied voltage changes, the high-potential cathode color-changing material will undergo an oxidation-reduction reaction with the anode color-changing material and then be used to adjust the transmittance of near-infrared light. Therefore, the electrochromic device made of the electrochromic material with adjustable visible light and near-infrared light transmittance according to the embodiment of the present application can adjust and control the transmittance of visible light and the transmittance of near-infrared light respectively. When the electrochromic device is used in a camera, it can adjust the transmittance of visible light to assist daytime imaging, and can adjust the transmittance of near-infrared light to assist night imaging.
[0051] In the electrochromic device made of the electrochromic material with adjustable visible light and near-infrared light transmittance according to the embodiment of the present application, since the redox potential of the high-potential cathode color-changing material is higher than the redox potential of the low-potential cathode color-changing material, in the present embodiment, when the voltage applied to the electrochromic device changes in the low voltage range of 0 to 1.2 V, the low-potential cathode color-changing material will first undergo a redox reaction with the anode color-changing material as the voltage changes, thereby being able to cause a significant change in the transmittance of visible light, that is, being able to have a better regulating effect on the transmittance of visible light, while the transmittance of near-infrared light will not change significantly at this time. When the voltage applied to the electrochromic device changes in the high voltage range of 1.2 to 2V, the high-potential cathode color-changing material will undergo an oxidation-reduction reaction with the anode color-changing material as the voltage changes, thereby causing the transmittance of near-infrared light to change significantly, that is, it can have a better regulating effect on the transmittance of near-infrared light. At this time, the low-potential cathode color-changing material has been reduced to a large extent, so the transmittance of visible light will not change significantly, thereby realizing the separate regulation of the visible light transmittance and the near-infrared light transmittance under different voltages.
[0052] Specifically, the molar ratio of the sum of the high-potential cathode color-changing material and the low-potential cathode color-changing material to the anode color-changing material is 1:1.
[0053] Specifically, the concentrations of the anode color-changing material, the high-potential cathode color-changing material and the low-potential cathode color-changing material are all 1 to 100 mM. Preferably, the concentration of the anode color-changing material is preferably 20 to 80 mM, the concentration of the high-potential cathode color-changing material is preferably 10 to 50 mM, and the concentration of the low-potential cathode color-changing material is preferably 10 to 50 mM. Among them, by adjusting the ratio and concentration of the high-potential cathode color-changing material and the low-potential cathode color-changing material, the adjustable contrast of the visible light region and the near-infrared light region can be controlled. If a large adjustment range is required in the visible light region, the ratio and concentration of the low-potential cathode color-changing material are increased, and if a large adjustment range is required in the near-infrared light region, the ratio and concentration of the high-potential cathode color-changing material are increased; wherein, the concentrations of the anode color-changing material, the high-potential cathode color-changing material and the low-potential cathode color-changing material are selected according to the contrast requirements in the visible light range.
[0054] Specifically, a combination of an anodic color-changing material, a high-potential cathode color-changing material and a low-potential cathode color-changing material is provided, wherein the anodic color-changing material is 1,1':4'1"-terphenyl-4,4"-dithiol, and has the structural formula:
[0055]
[0056] The high potential cathode color-changing material is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate, and the structural formula is:
[0057]
[0058] The low potential cathode color changing material is hexyl viologen bistetrafluoroborate, and the structural formula is:
[0059]
[0060] Specifically, another combination of an anode color-changing material, a high-potential cathode color-changing material, and a low-potential cathode color-changing material is provided, wherein the anode color-changing material is 5,10-diisopropyl-5,10-dihydrophenazine, and has the structural formula:
[0061]
[0062] The high potential cathode color-changing material is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate, and the structural formula is:
[0063]
[0064] The low potential cathode color-changing material is 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate), and the structural formula is:
[0065]
[0066] The present invention also provides a method for preparing the electrochromic material with adjustable visible light and near-infrared light transmittances as described above, the method comprising the following steps:
[0067] S1: Take appropriate amounts of anode color-changing material, high-potential cathode color-changing material and low-potential cathode color-changing material and mix them into a solution.
[0068] Specifically, the method also includes the following steps:
[0069] S0: Prepare anode color-changing materials, high-potential cathode color-changing materials and low-potential cathode color-changing materials.
[0070] Specifically, when the anode color-changing material is 1,1':4'1"-terphenyl-4,4"-dithiol, the high potential cathode color-changing material is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate, and the low potential cathode color-changing material is hexyl viologen bis-tetrafluoroborate, the specific operation of step S0 is as follows:
[0071] Wherein, the step of preparing the anode color changing material 1,1':4'1"-terphenyl-4,4"-dithiol in step S0 is:
[0072] M1: bromobenzene, phenylboric acid, Pd(OAc)2, potassium carbonate, DMF and water are added to a microwave reaction device and heated by microwave irradiation for reaction. After the reaction is completed, ethyl acetate is used to extract the product 1,1':4',1"-terphenyl from the reaction mixture. A mixture of ethyl acetate and n-hexane in a ratio of 1:1 is then used as an eluent to purify the extracted product 1,1':4',1"-terphenyl by column chromatography;
[0073] M2: Under a nitrogen atmosphere, chlorosulfonic acid and dichloromethane were added to the reaction vessel, and then the 1,1':4',1"-terphenyl obtained in step M1 was added dropwise, the reaction temperature was maintained at 0°C, and then the temperature was raised to room temperature and stirred. After the reaction was completed, a large amount of saturated brine was added to the system, and then the organic phase was extracted with dichloromethane and collected. The organic phase was then dried with MgSO4 and the solvent in the organic phase was removed by rotary evaporation, and then separated by column chromatography to obtain 1,1':4',1"-terphenyl-4,4"-disulfonyl chloride;
[0074] M3: Take the 1,1':4',1"-terphenyl-4,4"-disulfonyl chloride synthesized in step M2 and dissolve it in tetrahydrofuran solvent, add LiAlH4 and reflux reaction, add appropriate amount of ice water to quench after the reaction is completed, then add concentrated hydrochloric acid to adjust the pH value to less than or equal to 1, then filter to remove precipitated impurities, extract the solution with dichloromethane and collect the organic phase, then dry the organic phase with MgSO4 and spin dry the solvent in the organic phase to obtain light yellow crystalline 1,1':4'1"-terphenyl-4,4"-dithiol;
[0075] Wherein, the step of preparing the high potential cathode color-changing material (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate in step S0 is:
[0076] N1: Add dichloroethane, tetra-tert-butylferrocene and 6-bromohexanoyl chloride to a reaction vessel under nitrogen protection, cool the mixed solution in the reaction vessel to 0°C, then put AlCl3 into the reaction vessel, pour the reaction mixture into stirring water and stir after the reaction is completed, then add sufficient ether to form a stratification of the reaction mixture, then add concentrated hydrochloric acid and zinc powder to the system to ensure that the iron salt exists in a divalent form, collect the organic phase and the aqueous phase respectively with a separatory funnel after the reduction is completed, then add ether to the system to continue extraction and continue to collect the organic phase and the aqueous phase with a separatory funnel, then combine all the collected organic phases, wash the organic phase with an aqueous solution containing NaHCO3 and salt, then dry the organic phase with MgSO4, filter the organic phase, and then rotary evaporate to remove the solvent in the organic phase to obtain a red oily substance; add the red oily substance to a vacuum-assisted silica gel column and elute with n-hexane to remove residual ferrocene, and finally rotary evaporate the eluted product to remove the solvent to obtain 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone;
[0077] N2: Dissolve AlCl3 in dry ether and place in a Schlenk flask, cool the solution in the Schlenk flask to 0°C, inject LiAlH4 into the Schlenk flask with a syringe, and then heat the suspension obtained by the reaction to room temperature and stir; take 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone prepared in step N1 and add it to the Schlenk flask, then heat the reaction solution in the Schlenk flask to reflux and then cool to room temperature. After the reaction is completed, add the Schlenk flask to a flask and heat to reflux. nk flask, adding water to quench the reaction solution, then adding ether to extract the reaction solution and separating the organic phase with a separatory funnel, then washing the separated organic phase with an aqueous solution containing NaHCO3 and salt, and then drying with MgSO4, filtering and then removing the solvent in the organic phase by rotary evaporation to obtain a yellow-orange oil; adding the yellow-orange oil to a vacuum-assisted silica gel column and eluting with n-hexane to separate, and the product obtained after elution is separated by rotary evaporation to remove the solvent to obtain 6-bromo-1-(tetra-tert-butylferrocenylhexane);
[0078] N3: triethylamine, acetonitrile and 6-bromo-1-(tetra-tert-butylferrocenehexane) prepared in step N2 are added to a reaction container, the solution in the reaction container is heated to reflux for reaction, the solvent is removed by rotary evaporation after the reaction is cooled to room temperature to obtain a crude product, the crude product is washed with ether, filtered and then dried in a vacuum to obtain a bromide salt, the bromide salt is dissolved in methanol and an excess of NaBF4 aqueous solution is added to react, the methanol is removed by rotary evaporation from the solution obtained by the reaction to obtain an orange precipitate, the orange precipitate is collected on a filter element, repeatedly recrystallized, and stored for standby use; wherein the orange precipitate is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate;
[0079] Wherein, the step of preparing the low potential cathode color-changing material hexyl viologen bistetrafluoroborate in step S0 is:
[0080] Add 4-4'-bipyridine, 1-bromohexane and N,N'-dimethylformamide solvent to the reaction container and heat to reflux to react to obtain a precipitate. After the reaction is completed, cool to room temperature and collect the precipitate by vacuum filtration. Then, wash the collected precipitate with N,N'-dimethylformamide and acetone solvent respectively, and then vacuum dry the precipitate to obtain the product hexyl viologen bistetrafluoroborate.
[0081] Specifically, when the anode color-changing material is 5,10-diisopropyl-5,10-dihydrophenazine, the high potential cathode color-changing material is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate, and the low potential cathode color-changing material is 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate), the specific operation of step S0 is as follows:
[0082] The step of preparing the anode color-changing material 5,10-diisopropyl-5,10-dihydrophenazine in step S0 is as follows:
[0083] A finely ground metal alloy, phenazine and 1,2-dimethoxyethane in a potassium-sodium ratio of 10:1 are placed in a reaction vessel and stirred until a brick-red slurry is formed, then the stirring is stopped and the reaction is allowed to stand, then 2-bromopropane is added to the reaction mixture and stirred, after the reaction is completed, the precipitate in the reaction mixture is filtered out, and then the solvent in the reaction mixture is removed by rotary evaporation, and then a mixture of hexane and ethyl acetate in a ratio of 8:2 is used as an eluent to elute and separate the reaction mixture through a vacuum-assisted silica gel column to obtain a white solid, and the white solid is dissolved in methanol and recrystallized to obtain 5,10-diisopropyl-5,10-dihydrophenazine;
[0084] Wherein, the step of preparing the high potential cathode color-changing material (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate in step S0 is:
[0085] N1: Add dichloroethane, tetra-tert-butylferrocene and 6-bromohexanoyl chloride to a reaction vessel under nitrogen protection, cool the mixed solution in the reaction vessel to 0°C, then put AlCl3 into the reaction vessel, pour the reaction mixture into stirring water and stir after the reaction is completed, then add sufficient ether to form a stratification of the reaction mixture, then add concentrated hydrochloric acid and zinc powder to the system to ensure that the iron salt exists in a divalent form, collect the organic phase and the aqueous phase respectively with a separatory funnel after the reduction is completed, then add ether to the system to continue extraction and continue to collect the organic phase and the aqueous phase with a separatory funnel, then combine all the collected organic phases, wash the organic phase with an aqueous solution containing NaHCO3 and salt, then dry the organic phase with MgSO4, filter the organic phase, and then rotary evaporate to remove the solvent in the organic phase to obtain a red oily substance; add the red oily substance to a vacuum-assisted silica gel column and elute with n-hexane to remove residual ferrocene, and finally rotary evaporate the eluted product to remove the solvent to obtain 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone;
[0086] N2: Dissolve AlCl3 in dry ether and place in a Schlenk flask, cool the solution in the Schlenk flask to 0°C, inject LiAlH4 into the Schlenk flask with a syringe, and then heat the suspension obtained by the reaction to room temperature and stir; take 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone prepared in step N1 and add it to the Schlenk flask, then heat the reaction solution in the Schlenk flask to reflux and then cool to room temperature. After the reaction is completed, add the Schlenk flask to a flask and heat to reflux. nk flask, adding water to quench the reaction solution, then adding ether to extract the reaction solution and separating the organic phase with a separatory funnel, then washing the separated organic phase with an aqueous solution containing NaHCO3 and salt, and then drying with MgSO4, filtering and then removing the solvent in the organic phase by rotary evaporation to obtain a yellow-orange oil; adding the yellow-orange oil to a vacuum-assisted silica gel column and eluting with n-hexane to separate, and the product obtained after elution is separated by rotary evaporation to remove the solvent to obtain 6-bromo-1-(tetra-tert-butylferrocenylhexane);
[0087] N3: triethylamine, acetonitrile and 6-bromo-1-(tetra-tert-butylferrocenehexane) prepared in step N2 are added to a reaction container, the solution in the reaction container is heated to reflux for reaction, the solvent is removed by rotary evaporation after the reaction is cooled to room temperature to obtain a crude product, the crude product is washed with ether, filtered and then dried in a vacuum to obtain a bromide salt, the bromide salt is dissolved in methanol and an excess of NaBF4 aqueous solution is added to react, the methanol is removed by rotary evaporation from the solution obtained by the reaction to obtain an orange precipitate, the orange precipitate is collected on a filter element, repeatedly recrystallized, and stored for standby use; wherein the orange precipitate is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate;
[0088] The step of preparing the low potential cathode color changing material 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate) in step S0 is:
[0089] 3,5-dimethylaniline is added to a solution of dimethylformamide and water in a ratio of 3:2, and heated under a nitrogen atmosphere for reflux reaction. Then, 1,1'-di(2,4-dinitrophenyl)-4,4'-bipyridine is dissolved in water and added to the reaction solution through a constant pressure dropping funnel for reflux reaction. After the reaction is cooled, the yellow-brown precipitate produced is filtered out, and the water in the filtrate is removed by rotary evaporation to obtain a concentrated solution. Then, a large amount of acetone is added to the concentrated solution for reaction to obtain a yellow precipitate. After filtering and collecting the yellow precipitate, the yellow precipitate is dissolved in a small amount of water and an excess of NaBF4 is added for reaction to obtain an orange precipitate. The obtained orange precipitate is purified by repeated crystallization with methanol to obtain an off-white solid, which is 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate).
[0090] The present invention also provides an electrochromic device, comprising a device body, wherein the device body has an electrochromic layer, and the electrochromic layer comprises any one of the electrochromic materials with adjustable visible light and near-infrared light transmittances as described above.
[0091] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below based on specific embodiments.
[0092] Example 1
[0093] The electrochromic material with adjustable visible light and near-infrared light transmittance of the present embodiment is mainly formed by mixing an anodic color-changing material, a high-potential cathode color-changing material with an absorption peak in the near-infrared light wavelength range, and a low-potential cathode color-changing material with an absorption peak in the visible light wavelength range, wherein the redox potential of the high-potential cathode color-changing material is higher than that of the low-potential cathode color-changing material; wherein the molar ratio of the sum of the high-potential cathode color-changing material and the low-potential cathode color-changing material to the anodic color-changing material is 1:1, the anodic color-changing material is 45 molar parts of 1,1':4'1"-terphenyl-4,4"-dithiol, the high-potential cathode color-changing material is 15 molar parts of (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate, and the low-potential cathode color-changing material is 30 molar parts of hexyl viologen bis-tetrafluoroborate.
[0094] The steps of the preparation method are:
[0095] S0: Prepare anode color-changing materials, high-potential cathode color-changing materials and low-potential cathode color-changing materials.
[0096] S1: Take corresponding molar portions of an anodic color-changing material, a high-potential cathode color-changing material and a low-potential cathode color-changing material and mix them into a solution.
[0097] In this embodiment, the steps of preparing the anodic color changing material 1,1':4'1"-terphenyl-4,4"-dithiol in step S0 are:
[0098] M1: Bromobenzene (1 mmol), phenylboric acid (1 mmol), Pd(OAc)2 (1 mol%), potassium carbonate (2 mmol), DMF (3 mL) and water (3 mL) were added into a microwave reaction apparatus and heated at 100°C with microwave (300 W) for 5 min. After the reaction, ethyl acetate was used to extract the product 1,1':4',1"-terphenyl from the reaction mixture. A mixture of ethyl acetate and n-hexane in a ratio of 1:1 was used as an eluent and the extracted product 1,1':4',1"-terphenyl was purified by column chromatography.
[0099] M2: Under nitrogen atmosphere, chlorosulfonic acid (0.53 ml, 8 eq.) and dichloromethane (10 mL) were added to the reaction vessel, and then 1,1':4',1"-terphenyl (0.230 g, 1.0 mmol) obtained in step M1 was added dropwise, and the reaction temperature was maintained at 0°C, then the temperature was raised to room temperature and stirred for 6 hours. After the reaction was completed, a large amount of saturated brine was added to the system, and then the organic phase was extracted with dichloromethane and collected. The organic phase was then dried with MgSO4 and the solvent in the organic phase was removed by rotary evaporation, and then 1,1':4',1"-terphenyl-4,4"-disulfonyl chloride (0.288 g, 1.01 mmol, 67%) was obtained by column chromatography.
[0100] M3: Take 0.255g (0.90mmol) of 1,1':4',1"-terphenyl-4,4"-disulfonyl chloride synthesized in step M2 and dissolve it in tetrahydrofuran solvent (30mL), add LiAlH4 (1.518g, 40mmol) and reflux for 3 hours, add appropriate amount of ice water to quench after the reaction is completed, then add concentrated hydrochloric acid to adjust the pH value to less than or equal to 1, then filter to remove precipitated impurities, extract the solution with dichloromethane and collect the organic phase, then dry the organic phase with MgSO4 and spin dry the solvent in the organic phase to obtain light yellow crystals 1,1':4'1"-terphenyl-4,4"-dithiol (0.904g, 3.07mmol, 51% yield);
[0101] Specifically, repeat the above steps M1 to M3 to prepare a sufficient amount of 1,1':4'1"-terphenyl-4,4"-dithiol;
[0102] In this embodiment, the steps of preparing the high potential cathode color-changing material (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate in step S0 are:
[0103] N1: 350 mL of ethylene dichloride, 50.0 g (122 mmol) of tetra-tert-butylferrocene and 19.3 mL (126 mmol) of 6-bromohexanoyl chloride were added to the reaction vessel under nitrogen protection. The mixed solution in the reaction vessel was cooled to 0°C, and then 13.3 g (100 mmol) of AlCl3 was divided into 3 equal parts and added to the reaction vessel at intervals of 2 hours each. After the reaction was completed, the reaction mixture was poured into 300 mL of water and stirred, and then a sufficient amount of ether was added to form a stratified reaction mixture. Then, 50 mL of concentrated hydrochloric acid and 2 to 5 g of zinc powder were added to the system to ensure that the iron salt was present in a divalent form. After the reduction was completed, After the mixture is completed, the organic phase and the aqueous phase are collected separately with a separatory funnel, and then 200 mL of ether is added to the system to continue extraction and the organic phase and the aqueous phase are continued to be collected with a separatory funnel, and then all the collected organic phases are combined, and the organic phase is washed with an aqueous solution containing NaHCO3 and salt, and then the organic phase is dried with MgSO4, and then the organic phase is filtered and then the solvent in the organic phase is removed by rotary evaporation to obtain a red oily substance; the red oily substance is added to a vacuum-assisted silica gel column and eluted with n-hexane to remove residual ferrocene, and finally the eluted product is subjected to rotary evaporation to remove the solvent to obtain 64.29 g of 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone;
[0104] N2: 2.27 g (17.02 mmol) of AlCl3 was dissolved in 200 mL of dry ether and placed in a Schlenk flask. The solution in the Schlenk flask was cooled to 0°C. 0.65 g (17.0 mmol) of LiAlH4 was injected into the Schlenk flask with a syringe. The resulting suspension was heated to room temperature and stirred for 15 min. 10.0 g (17.02 mmol) of 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone prepared in step N1 was added to the Schlenk flask. The reaction solution was heated to reflux for 3 hours and then cooled to room temperature. After the reaction was completed, water was added to the reaction solution in the Schlenk flask to quench it, and then ether was added to extract the reaction solution and the organic phase was separated by a separatory funnel. The separated organic phase was then washed with an aqueous solution containing NaHCO3 and salt, and then dried with MgSO4. After filtering, the solvent in the organic phase was removed by rotary evaporation to obtain a yellow-orange oily substance; the yellow-orange oily substance was added to a vacuum-assisted silica gel column and eluted and separated with n-hexane, and the product obtained after elution was subjected to rotary evaporation to remove the solvent and separate 8.73 g of 6-bromo-1-(tetra-tert-butylferrocenylhexane);
[0105] N3: 16.5 mL (105 mmol) of triethylamine, 20 mL of acetonitrile and 8.73 g (25.0 mmol) of 6-bromo-1-(tetra-tert-butylferrocenehexane) prepared in step N2 were added to a reaction vessel, and the solution in the reaction vessel was heated to reflux for reaction for 4 days. After the reaction was cooled to room temperature, the solvent was removed by rotary evaporation to obtain a crude product, and the crude product was washed with ether, filtered, and then dried in a vacuum to obtain a bromide salt, and the bromide salt was dissolved in methanol and an excess of NaBF4 aqueous solution was added to react, and the solution obtained by the reaction was subjected to rotary evaporation to remove methanol to obtain an orange precipitate, and the orange precipitate was collected on a filter element, repeatedly recrystallized, and stored for standby use; wherein the orange precipitate is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate;
[0106] Specifically, repeat the above steps N1 to N3 to prepare a sufficient amount of (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate;
[0107] In this embodiment, the steps of preparing the low potential cathode color-changing material hexyl viologen bistetrafluoroborate in step S0 are:
[0108] 0.31 g (2 mmol) of 4-4' bipyridine, 0.82 g (5 mmol) of 1-bromohexane and 8.0 mL of N, N'-dimethylformamide solvent were added to the reaction container and heated to 120°C for reflux reaction for 30 min to obtain a precipitate. After the reaction was completed, the precipitate was cooled to room temperature and collected by vacuum filtration. The collected precipitate was washed three times with N, N'-dimethylformamide and acetone solvent respectively, and then the precipitate was vacuum dried to obtain the product hexyl viologen bistetrafluoroborate;
[0109] Specifically, the above steps are repeated to prepare a sufficient amount of hexyl viologen bistetrafluoroborate.
[0110] The transmittance test of the electrochromic material prepared in Example 1 was carried out, and the test steps were as follows:
[0111] Two pieces of 40 mm×40 mm×0.4 mm ITO-plated conductive glass were glued together at different positions to form a box body with a thickness of 125 μm. The electrochromic material prepared in Example 1 was filled into the box body by vacuum filling. A voltage varying between 0 and 2 V was applied to both ends of the box body, and the transmittance of light in the 550 nm band and the 940 nm band passing through the box body was measured.
[0112] The transmittance test of Example 1 was performed for 10 groups and the average transmittance was recorded in Table 1;
[0113] The guide surfaces of the two sheets of conductive glass in the box body are arranged opposite to each other, and the box thickness is the thickness of the gap between the two sheets of conductive glass, and the gap is used to fill the electrochromic material.
[0114] Example 2
[0115] The electrochromic material with adjustable visible light and near-infrared light transmittance of the present embodiment is mainly formed by mixing an anodic color-changing material, a high-potential cathode color-changing material with an absorption peak in the near-infrared light wavelength range, and a low-potential cathode color-changing material with an absorption peak in the visible light wavelength range, wherein the redox potential of the high-potential cathode color-changing material is higher than that of the low-potential cathode color-changing material; wherein the molar ratio of the sum of the high-potential cathode color-changing material and the low-potential cathode color-changing material to the anodic color-changing material is 1:1, the anodic color-changing material is 45 molar parts of 5,10-diisopropyl-5,10-dihydrophenazine, the high-potential cathode color-changing material is 20 molar parts of (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate, and the low-potential cathode color-changing material is 25 molar parts of 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate).
[0116] The steps of the preparation method are:
[0117] S0: Prepare anode color-changing materials, high-potential cathode color-changing materials and low-potential cathode color-changing materials.
[0118] S1: Take corresponding molar portions of an anodic color-changing material, a high-potential cathode color-changing material and a low-potential cathode color-changing material and mix them into a solution.
[0119] In this embodiment, the steps of preparing the anode color-changing material 5,10-diisopropyl-5,10-dihydrophenazine in step S0 are:
[0120] 6.5 g of a finely ground metal alloy with a potassium-sodium ratio of 10:1, 9.0 g of phenazine and 150 mL of 1,2-dimethoxyethane were placed in a reaction vessel and stirred at 40°C until a brick-red slurry was formed, then the stirring was stopped and the reaction was allowed to stand for 24 hours, then 14.1 mL of 2-bromopropane was added to the reaction mixture and stirred for 2 hours, after the reaction was completed, the precipitate in the reaction mixture was filtered out, and the solvent in the reaction mixture was removed by rotary evaporation, and then a mixture of hexane and ethyl acetate in a ratio of 8:2 was used as an eluent to elute and separate the reaction mixture through a vacuum-assisted silica gel column to obtain a white solid, and the white solid was dissolved in methanol and recrystallized to obtain 2.1 g of 5,10-diisopropyl-5,10-dihydrophenazine;
[0121] Specifically, the above steps are repeated to prepare a sufficient amount of 5,10-diisopropyl-5,10-dihydrophenazine;
[0122] In this embodiment, the steps of preparing the high potential cathode color-changing material (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate in step S0 are:
[0123] N1: 350 mL of ethylene dichloride, 50.0 g (122 mmol) of tetra-tert-butylferrocene and 19.3 mL (126 mmol) of 6-bromohexanoyl chloride were added to the reaction vessel under nitrogen protection. The mixed solution in the reaction vessel was cooled to 0°C. Then 13.3 g (100 mmol) of AlCl3 was divided into 3 equal parts and added to the reaction vessel at intervals of 2 hours each. After the reaction was completed, the reaction mixture was poured into 300 mL of stirring water and stirred. Then, sufficient ether was added to form a stratified layer in the reaction mixture. Then, 50 mL of concentrated hydrochloric acid and 2 to 5 g of zinc powder were added to the system to ensure that the iron salt was present in a divalent form. After reduction, After completion, the organic phase and the aqueous phase were collected separately with a separatory funnel, and then 200 mL of ether was added to the system to continue extraction and the organic phase and the aqueous phase were continued to be collected with a separatory funnel, and then all the collected organic phases were combined, and the organic phase was washed with an aqueous solution containing NaHCO3 and salt, and then the organic phase was dried with MgSO4, and then the organic phase was filtered and then rotary evaporated to remove the solvent in the organic phase and obtain a red oily substance; the red oily substance was added to a vacuum-assisted silica gel column and eluted with n-hexane to remove residual ferrocene, and finally the eluted product was subjected to rotary evaporation to remove the solvent to obtain 64.29 g of 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone;
[0124] N2: 2.27 g (17.02 mmol) of AlCl3 was dissolved in 200 mL of dry ether and placed in a Schlenk flask. The solution in the Schlenk flask was cooled to 0°C. 0.65 g (17.0 mmol) of LiAlH4 was injected into the Schlenk flask with a syringe. The resulting suspension was heated to room temperature and stirred for 15 min. 10.0 g (17.02 mmol) of 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone prepared in step N1 was added to the Schlenk flask. The reaction solution was heated to reflux for 3 hours and then cooled to room temperature. After the reaction was completed, water was added to the reaction solution in the Schlenk flask to quench it, and then ether was added to extract the reaction solution and the organic phase was separated by a separatory funnel. The separated organic phase was then washed with an aqueous solution containing NaHCO3 and salt, and then dried with MgSO4. After filtering, the solvent in the organic phase was removed by rotary evaporation to obtain a yellow-orange oily substance; the yellow-orange oily substance was added to a vacuum-assisted silica gel column and eluted and separated with n-hexane, and the product obtained after elution was subjected to rotary evaporation to remove the solvent and separate 8.73 g of 6-bromo-1-(tetra-tert-butylferrocenylhexane);
[0125] N3: 16.5 mL (105 mmol) of triethylamine, 20 mL of acetonitrile and 8.73 g (25.0 mmol) of 6-bromo-1-(tetra-tert-butylferrocenehexane) prepared in step N2 were added to a reaction vessel, and the solution in the reaction vessel was heated to reflux for reaction for 4 days. After the reaction was cooled to room temperature, the solvent was removed by rotary evaporation to obtain a crude product, and the crude product was washed with ether, filtered, and then dried in a vacuum to obtain a bromide salt, and the bromide salt was dissolved in methanol and an excess of NaBF4 aqueous solution was added to react, and the solution obtained by the reaction was subjected to rotary evaporation to remove methanol to obtain an orange precipitate, and the orange precipitate was collected on a filter element, repeatedly recrystallized, and stored for standby use; wherein the orange precipitate is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate;
[0126] Specifically, repeat the above steps N1 to N3 to prepare a sufficient amount of (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate;
[0127] In this embodiment, the steps of preparing the low potential cathode color-changing material 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate) in step S0 are:
[0128] 6.7 mL of 3,5-dimethylaniline was added to 30 mL of a solution of dimethylformamide and water in a ratio of 3:2, and the mixture was heated to reflux reaction under a nitrogen atmosphere. Then 5.0 g of 1,1'-di(2,4-dinitrophenyl)-4,4'-bipyridine was dissolved in 50 mL of water and slowly added to the reaction solution through a constant pressure dropping funnel and then refluxed for 5 hours. After the reaction was cooled, the yellow-brown precipitate was filtered out, and the water in the filtrate was removed by rotary evaporation to obtain a concentrated solution, and then the concentrated solution was added to the reaction mixture. A large amount of acetone is added to react to obtain a yellow precipitate, and the yellow precipitate is collected by filtration, dissolved in a small amount of water, and an excess of NaBF4 is added to react to obtain an orange precipitate. The obtained orange precipitate is repeatedly crystallized and purified by methanol to obtain an off-white solid, which is 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate); specifically, the above steps are repeated to prepare a sufficient amount of 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate).
[0129] The transmittance test of the electrochromic material prepared in Example 2 was carried out, and the test steps were as follows:
[0130] Two pieces of 40 mm×40 mm×0.4 mm ITO-plated conductive glass were glued together at different positions to form a box body with a thickness of 125 μm. The electrochromic material prepared in Example 2 was filled into the box body by vacuum filling. A voltage varying between 0 and 2 V was applied to both ends of the box body, and the transmittance of light in the 550 nm band and the 940 nm band passing through the box body was measured.
[0131] The transmittance test of Example 2 was performed for 10 groups and the average transmittance was recorded in Table 1;
[0132] The guide surfaces of the two sheets of conductive glass in the box body are arranged opposite to each other, and the box thickness is the thickness of the gap between the two sheets of conductive glass, and the gap is used to fill the electrochromic material.
[0133] Example 3
[0134] An electrochromic device comprises a device body, wherein the device body has an electrochromic layer, and the electrochromic layer comprises the electrochromic material with adjustable visible light and near-infrared light transmittances as prepared in Example 1.
[0135] Example 4
[0136] Another electrochromic device comprises a device body, wherein the device body has an electrochromic layer, and the electrochromic layer comprises the electrochromic material with adjustable visible light and near-infrared light transmittance as prepared in Example 2.
[0137] Comparative Example 1
[0138] Purchase the electrochromic materials available on the market and conduct a transmittance test on the electrochromic materials purchased on the market. The test steps are as follows:
[0139] Two pieces of 40mm×40mm×0.4mm ITO-plated conductive glass were glued together at different positions to form a box body with a thickness of 125μm. The electrochromic material purchased on the market was filled into the box body by vacuum filling. A voltage varying between 0 and 2V was applied to both ends of the box body, and the transmittance of light in the 550nm band and the 940nm band passing through the box body was measured.
[0140] The transmittance test of Comparative Example 1 was carried out for 10 groups and the average transmittance was recorded in Table 1;
[0141] The guide surfaces of the two sheets of conductive glass in the box body are arranged opposite to each other, and the box thickness is the thickness of the gap between the two sheets of conductive glass, and the gap is used to fill the electrochromic material.
[0142] Table 1
[0143]
[0144] As can be seen from the data in Table 1, the electrochromic material with adjustable visible light-near infrared light transmittance in the embodiment of the present application can adjust both the transmittance of visible light and the transmittance of near infrared light. When the applied voltage changes in the low voltage range of 0 to 1.2V, the low potential cathode discoloration material will first undergo an oxidation-reduction reaction with the anode discoloration material as the voltage changes, thereby enabling the transmittance of visible light to change significantly, that is, it can have a better regulating effect on the transmittance of visible light, while the transmittance of near infrared light will not change significantly at this time. When the applied voltage changes in the high voltage range of 1.2 to 2V, the high potential cathode discoloration material will undergo an oxidation-reduction reaction with the anode discoloration material as the voltage changes, thereby enabling the transmittance of near infrared light to change significantly, that is, it can have a better regulating effect on the transmittance of near infrared light, while the low potential cathode discoloration material has been reduced more at this time, so the transmittance of visible light will not change significantly, thereby achieving the separate regulation of the transmittance of visible light and the transmittance of near infrared light at different voltages. The existing electrochromic materials purchased on the market have a significant change in transmittance in the visible light band as the voltage changes, so they have a good regulating effect on the transmittance of visible light. However, the transmittance in the near-infrared light band changes less, and cannot produce a good regulating effect on the transmittance of near-infrared light. The specific embodiments described above further explain in detail the technical problems, technical solutions and beneficial effects solved by the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An electrochromic material with adjustable visible light and near-infrared light transmittance, characterized in that: It is mainly formed by mixing an anode color-changing material, a high-potential cathode color-changing material whose absorption peak is in the near-infrared light wavelength range, and a low-potential cathode color-changing material whose absorption peak is in the visible light wavelength range; wherein the redox potential of the high-potential cathode color-changing material is higher than that of the low-potential cathode color-changing material.
2. The electrochromic material with adjustable visible light and near infrared light transmittance according to claim 1, characterized in that: The molar ratio of the sum of the high potential cathode color-changing material and the low potential cathode color-changing material to the anode color-changing material is 1:
1.
3. The electrochromic material with adjustable visible light and near infrared light transmittance according to claim 1, characterized in that: The concentrations of the anode color-changing material, the high-potential cathode color-changing material and the low-potential cathode color-changing material are all 1 to 100 mM.
4. The electrochromic material with adjustable visible light and near infrared light transmittance according to claim 1, characterized in that: The anode color-changing material is 1,1':4'1"-terphenyl-4,4"-dithiol, and the structural formula is: The high potential cathode color-changing material is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate, and the structural formula is: The low potential cathode color changing material is hexyl viologen bistetrafluoroborate, and the structural formula is:
5. The electrochromic material with adjustable visible light and near infrared light transmittance according to claim 1, characterized in that: The anode color-changing material is 5,10-diisopropyl-5,10-dihydrophenazine, and the structural formula is: The high potential cathode color-changing material is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate, and the structural formula is: The low potential cathode color-changing material is 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate), and the structural formula is:
6. A method for preparing an electrochromic material with adjustable visible light and near infrared light transmittance as claimed in any one of claims 1 to 3, characterized in that: The steps of the method include: S1: Take appropriate amounts of anode color-changing material, high-potential cathode color-changing material and low-potential cathode color-changing material and mix them into a solution.
7. The preparation method according to claim 6, characterized in that: The method also includes the following steps: S0: Prepare anode color-changing materials, high-potential cathode color-changing materials and low-potential cathode color-changing materials.
8. The preparation method according to claim 7, characterized in that: The anode color-changing material is 1,1':4'1"-terphenyl-4,4"-dithiol; The high potential cathode color-changing material is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate; The low potential cathode color changing material is hexyl viologen bistetrafluoroborate; Wherein, the step of preparing the anode color changing material 1,1':4'1"-terphenyl-4,4"-dithiol in step S0 is: M1: bromobenzene, phenylboric acid, Pd(OAc)2, potassium carbonate, DMF and water are added to a microwave reaction device and heated by microwave irradiation for reaction. After the reaction is completed, ethyl acetate is used to extract the product 1,1':4',1"-terphenyl from the reaction mixture. A mixture of ethyl acetate and n-hexane in a ratio of 1:1 is then used as an eluent to purify the extracted product 1,1':4',1"-terphenyl by column chromatography; M2: Under a nitrogen atmosphere, chlorosulfonic acid and dichloromethane were added to the reaction vessel, and then the 1,1':4',1"-terphenyl obtained in step M1 was added dropwise, the reaction temperature was maintained at 0°C, and then the temperature was raised to room temperature and stirred. After the reaction was completed, a large amount of saturated brine was added to the system, and then the organic phase was extracted with dichloromethane and collected. The organic phase was then dried with MgSO4 and the solvent in the organic phase was removed by rotary evaporation, and then separated by column chromatography to obtain 1,1':4',1"-terphenyl-4,4"-disulfonyl chloride; M3: Take the 1,1':4',1"-terphenyl-4,4"-disulfonyl chloride synthesized in step M2 and dissolve it in tetrahydrofuran solvent, add LiAlH4 and reflux reaction, add appropriate amount of ice water to quench after the reaction is completed, then add concentrated hydrochloric acid to adjust the pH value to less than or equal to 1, then filter to remove precipitated impurities, extract the solution with dichloromethane and collect the organic phase, then dry the organic phase with MgSO4 and spin dry the solvent in the organic phase to obtain light yellow crystalline 1,1':4'1"-terphenyl-4,4"-dithiol; Wherein, the step of preparing the high potential cathode color-changing material (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate in step S0 is: N1: Add dichloroethane, tetra-tert-butylferrocene and 6-bromohexanoyl chloride to a reaction vessel under nitrogen protection, cool the mixed solution in the reaction vessel to 0°C, then put AlCl3 into the reaction vessel, pour the reaction mixture into stirring water and stir after the reaction is completed, then add sufficient ether to form a stratification of the reaction mixture, then add concentrated hydrochloric acid and zinc powder to the system to ensure that the iron salt exists in a divalent form, collect the organic phase and the aqueous phase respectively with a separatory funnel after the reduction is completed, then add ether to the system to continue extraction and continue to collect the organic phase and the aqueous phase with a separatory funnel, then combine all the collected organic phases, wash the organic phase with an aqueous solution containing NaHCO3 and salt, then dry the organic phase with MgSO4, filter the organic phase, and then rotary evaporate to remove the solvent in the organic phase to obtain a red oily substance; add the red oily substance to a vacuum-assisted silica gel column and elute with n-hexane to remove residual ferrocene, and finally rotary evaporate the eluted product to remove the solvent to obtain 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone; N2: Dissolve AlCl3 in dry ether and place in a Schlenk flask, cool the solution in the Schlenk flask to 0°C, inject LiAlH4 into the Schlenk flask with a syringe, and then heat the suspension obtained by the reaction to room temperature and stir; take 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone prepared in step N1 and add it to the Schlenk flask, then heat the reaction solution in the Schlenk flask to reflux and then cool to room temperature. After the reaction is completed, add the Schlenk flask to a flask and heat to reflux. nk flask, adding water to quench the reaction solution, then adding ether to extract the reaction solution and separating the organic phase with a separatory funnel, then washing the separated organic phase with an aqueous solution containing NaHCO3 and salt, and then drying with MgSO4, filtering and then removing the solvent in the organic phase by rotary evaporation to obtain a yellow-orange oil; adding the yellow-orange oil to a vacuum-assisted silica gel column and eluting with n-hexane to separate, and the product obtained after elution is separated by rotary evaporation to remove the solvent to obtain 6-bromo-1-(tetra-tert-butylferrocenylhexane); N3: triethylamine, acetonitrile and 6-bromo-1-(tetra-tert-butylferrocenehexane) prepared in step N2 are added to a reaction container, the solution in the reaction container is heated to reflux for reaction, the solvent is removed by rotary evaporation after the reaction is cooled to room temperature to obtain a crude product, the crude product is washed with ether, filtered and then dried in a vacuum to obtain a bromide salt, the bromide salt is dissolved in methanol and an excess of NaBF4 aqueous solution is added to react, the methanol is removed by rotary evaporation from the solution obtained by the reaction to obtain an orange precipitate, the orange precipitate is collected on a filter element, repeatedly recrystallized, and stored for standby use; wherein the orange precipitate is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate; Wherein, the step of preparing the low potential cathode color-changing material hexyl viologen bistetrafluoroborate in step S0 is: Add 4-4'-bipyridine, 1-bromohexane and N,N'-dimethylformamide solvent to the reaction container and heat to reflux to react to obtain a precipitate. After the reaction is completed, cool to room temperature and collect the precipitate by vacuum filtration. Then, wash the collected precipitate with N,N'-dimethylformamide and acetone solvent respectively, and then vacuum dry the precipitate to obtain the product hexyl viologen bistetrafluoroborate.
9. The preparation method according to claim 7, characterized in that: The anode color-changing material is 5,10-diisopropyl-5,10-dihydrophenazine; The high potential cathode color-changing material is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate; The low potential cathode color-changing material is 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate); The step of preparing the anode color-changing material 5,10-diisopropyl-5,10-dihydrophenazine in step S0 is as follows: A finely ground metal alloy, phenazine and 1,2-dimethoxyethane in a potassium-sodium ratio of 10:1 are placed in a reaction vessel and stirred until a brick-red slurry is formed, then the stirring is stopped and the reaction is allowed to stand, then 2-bromopropane is added to the reaction mixture and stirred, after the reaction is completed, the precipitate in the reaction mixture is filtered out, and then the solvent in the reaction mixture is removed by rotary evaporation, and then a mixture of hexane and ethyl acetate in a ratio of 8:2 is used as an eluent to elute and separate the reaction mixture through a vacuum-assisted silica gel column to obtain a white solid, and the white solid is dissolved in methanol and recrystallized to obtain 5,10-diisopropyl-5,10-dihydrophenazine; Wherein, the step of preparing the high potential cathode color-changing material (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate in step S0 is: N1: Add dichloroethane, tetra-tert-butylferrocene and 6-bromohexanoyl chloride to a reaction vessel under nitrogen protection, cool the mixed solution in the reaction vessel to 0°C, then put AlCl3 into the reaction vessel, pour the reaction mixture into stirring water and stir after the reaction is completed, then add sufficient ether to form a stratification of the reaction mixture, then add concentrated hydrochloric acid and zinc powder to the system to ensure that the iron salt exists in a divalent form, collect the organic phase and the aqueous phase respectively with a separatory funnel after the reduction is completed, then add ether to the system to continue extraction and continue to collect the organic phase and the aqueous phase with a separatory funnel, then combine all the collected organic phases, wash the organic phase with an aqueous solution containing NaHCO3 and salt, then dry the organic phase with MgSO4, filter the organic phase, and then rotary evaporate to remove the solvent in the organic phase to obtain a red oily substance; add the red oily substance to a vacuum-assisted silica gel column and elute with n-hexane to remove residual ferrocene, and finally rotary evaporate the eluted product to remove the solvent to obtain 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone; N2: Dissolve AlCl3 in dry ether and place in a Schlenk flask, cool the solution in the Schlenk flask to 0°C, inject LiAlH4 into the Schlenk flask with a syringe, and then heat the suspension obtained by the reaction to room temperature and stir; take 6-bromo-1-(tetra-tert-butylferrocene)-2-hexanone prepared in step N1 and add it to the Schlenk flask, then heat the reaction solution in the Schlenk flask to reflux and then cool to room temperature. After the reaction is completed, add the Schlenk flask to a flask and heat to reflux. nk flask, adding water to quench the reaction solution, then adding ether to extract the reaction solution and separating the organic phase with a separatory funnel, then washing the separated organic phase with an aqueous solution containing NaHCO3 and salt, and then drying with MgSO4, filtering and then removing the solvent in the organic phase by rotary evaporation to obtain a yellow-orange oil; adding the yellow-orange oil to a vacuum-assisted silica gel column and eluting with n-hexane to separate, and the product obtained after elution is separated by rotary evaporation to remove the solvent to obtain 6-bromo-1-(tetra-tert-butylferrocenylhexane); N3: triethylamine, acetonitrile and 6-bromo-1-(tetra-tert-butylferrocenehexane) prepared in step N2 are added to a reaction container, the solution in the reaction container is heated to reflux for reaction, the solvent is removed by rotary evaporation after the reaction is cooled to room temperature to obtain a crude product, the crude product is washed with ether, filtered and then dried in a vacuum to obtain a bromide salt, the bromide salt is dissolved in methanol and an excess of NaBF4 aqueous solution is added to react, the methanol is removed by rotary evaporation from the solution obtained by the reaction to obtain an orange precipitate, the orange precipitate is collected on a filter element, repeatedly recrystallized, and stored for standby use; wherein the orange precipitate is (6-(tetra-tert-butylferrocene)hexyl)triethylamine-bis-tetrafluoroborate; The step of preparing the low potential cathode color changing material 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate) in step S0 is: 3,5-dimethylaniline is added to a solution of dimethylformamide and water in a ratio of 3:2, and heated under a nitrogen atmosphere for reflux reaction. Then, 1,1'-di(2,4-dinitrophenyl)-4,4'-bipyridine is dissolved in water and added to the reaction solution through a constant pressure dropping funnel for reflux reaction. After the reaction is cooled, the yellow-brown precipitate produced is filtered out, and the water in the filtrate is removed by rotary evaporation to obtain a concentrated solution. Then, a large amount of acetone is added to the concentrated solution for reaction to obtain a yellow precipitate. After filtering and collecting the yellow precipitate, the yellow precipitate is dissolved in a small amount of water and an excess of NaBF4 is added for reaction to obtain an orange precipitate. The obtained orange precipitate is purified by repeated crystallization with methanol to obtain an off-white solid, which is 1,1'-(3,5-dimethylphenyl)-4,4'-bipyridine (tetrafluoroborate).
10. An electrochromic device, characterized in that: The device comprises a device body, wherein the device body has an electrochromic layer, wherein the electrochromic layer comprises the electrochromic material with adjustable visible light and near-infrared light transmittance as claimed in any one of claims 1 to 5 or the electrochromic material prepared by the preparation method as claimed in any one of claims 6 to 9.
Citation Information
Cited By
Electrochromic intelligent window capable of accurately regulating and controlling mode as well as preparation method and application of electrochromic intelligent window
CN120010162A
Electrochromic composition capable of completely fading and application thereof
CN120590933A
Able to be completely faded electrochromic composition and its application
CN120590933B