Fluorescent material with good water resistance and preparation process thereof

By using the core-shell structure of modified phosphors in fluorescent materials, the phosphor is coated to improve aging resistance and water resistance, and the problem of good water resistance but poor aging resistance of organic fluorescent glue preparation materials is solved, and the long-term material is realized Stability and performance improvements.

CN119020023APending Publication Date: 2024-11-26HUAZHONG XINSHENG (TANGSHAN) FLUORESCENT MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411236173.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-26

Smart Images

  • Figure CN119020023A_ABST
    Figure CN119020023A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of fluorescent materials, and provides a fluorescent material with good water resistance and a preparation process thereof. A fluorescent material with good water resistance comprises organic fluorescent glue and modified fluorescent powder, the modified fluorescent powder is of a core-shell structure, the core in the core-shell structure is mesoporous silica microspheres doped with fluorescent powder, and the shell in the core-shell structure is a hydroxyl-containing compound, an isocyanate-group-containing compound and polystyrene. According to the technical scheme, the problem that a fluorescent material prepared from organic fluorescent glue in related technologies is good in water resistance but poor in aging resistance is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluorescent materials, and in particular to a fluorescent material with good water resistance and a preparation process thereof. Background Art

[0002] Fluorescent materials are substances that can emit visible light under the stimulation of ultraviolet rays or other radiation. According to the chemical composition and physical properties, they can be divided into inorganic fluorescent materials and organic fluorescent materials. Inorganic fluorescent materials are widely used because of their strong absorption capacity, high conversion rate, and stable physical and chemical properties.

[0003] Fluorescent materials have a wide range of applications in various fields due to their special luminescent properties, such as fluorescent lamps, LEDs, etc. With the continuous advancement of science and technology, people are also continuously deepening their research on fluorescent materials, striving to improve the stability of fluorescent materials to the external environment.

[0004] A Chinese invention patent with application number 202111027382.3 discloses an aging-resistant and anti-precipitation fluorescent material. The fluorescent powder is treated with gas-phase silica, an amino-containing alkaline solution, porous silica microspheres and a silane coupling agent, and then mixed with fluorescent glue to prepare an aging-resistant and anti-precipitation fluorescent material. The fluorescent glue uses inorganic fluorescent glue, which has good aging resistance but poor water resistance, and organic fluorescent glue has excellent water resistance but poor aging resistance. Summary of the invention

[0005] The invention provides a fluorescent material with good water resistance and a preparation process thereof, which solves the problem that the fluorescent material prepared by organic fluorescent glue in the related art has good water resistance but poor aging resistance.

[0006] The technical solution of the present invention is as follows: A fluorescent material with good water resistance comprises an organic fluorescent glue and a modified fluorescent powder, wherein the modified fluorescent powder is a core-shell structure, the core of the core-shell structure is a mesoporous silica microsphere doped with fluorescent powder, and the shell of the core-shell structure is a compound containing a hydroxyl group, a compound containing an isocyanate group and polystyrene.

[0007] As a further technical solution, the organic fluorescent glue can be any type of organic fluorescent glue, preferably Dow Corning OE-6351.

[0008] As a further technical solution, the phosphor may be any type of phosphor, preferably one or both of yttrium aluminum garnet phosphor and γ-phase alumina.

[0009] As a further technical solution, the mass ratio of the compound containing a hydroxyl group and the compound containing an isocyanate group to the polystyrene is 0.1 to 1:2.

[0010] As a further technical solution, the mass ratio of the compound containing a hydroxyl group and the compound containing an isocyanate group to the polystyrene is 0.5:2.

[0011] The present invention limits the mass ratio of the compound containing a hydroxyl group and the compound containing an isocyanate group to polystyrene to 0.5:2, thereby further improving the aging resistance and water resistance of the fluorescent material.

[0012] As a further technical solution, the mass ratio of the compound containing a hydroxyl group to the compound containing an isocyanate group is 0.1-0.4:0.4-0.1.

[0013] As a further technical solution, the mass ratio of the compound containing a hydroxyl group to the compound containing an isocyanate group is 1:1.

[0014] The present invention limits the mass ratio of the compound containing a hydroxyl group to the compound containing an isocyanate group to 1:1, thereby further improving the aging resistance and water resistance of the fluorescent material.

[0015] As a further technical solution, the compound containing an isocyanate group is a compound containing two or more isocyanate groups.

[0016] The present invention limits the compound containing an isocyanate group to a compound containing two or more isocyanate groups, thereby further improving the aging resistance and water resistance of the fluorescent material.

[0017] As a further technical solution, the compound containing an isocyanate group is a compound containing two isocyanate groups.

[0018] The present invention limits the compound containing an isocyanate group to a compound containing two isocyanate groups, thereby further improving the aging resistance and water resistance of the fluorescent material.

[0019] The compound containing two isocyanate groups in the present invention may be any compound containing two isocyanate groups, and is preferably hexamethylene diisocyanate.

[0020] As a further technical solution, the compound containing hydroxyl group is 1,4-cyclohexanedimethanol.

[0021] As a further technical solution, the mass ratio of the raw material of the core to the raw material of the shell is 30~35:2~3.

[0022] As a further technical solution, the raw materials of the core include phosphor and mesoporous silica microspheres in a mass ratio of 30:3-4.

[0023] The present invention limits the raw materials of the core to phosphor and mesoporous silica microspheres in a mass ratio of 30:3-4, thereby further improving the aging resistance and water resistance of the fluorescent material.

[0024] The present invention also provides a method for preparing a fluorescent material with good water resistance, comprising the following steps: S1, mixing the phosphor, mesoporous silica microspheres and solvent uniformly, filtering, washing and drying to obtain pretreated phosphor; S2, uniformly mixing the pretreated phosphor, the compound containing a hydroxyl group, the compound containing an isocyanate group, polystyrene and a solvent, filtering and drying to obtain a modified phosphor; S3, mixing the modified fluorescent powder and the organic fluorescent glue evenly to obtain a fluorescent material.

[0025] As a further technical solution, the solvent in S1 is an alcohol solution, preferably ethanol.

[0026] As a further technical solution, the solvent in S2 is N,N-dimethylformamide, and the mixing temperature is 15-20°C; the temperature is raised to 25-30°C before drying and kept warm for 20-40 minutes.

[0027] The working principle and beneficial effects of the present invention are: The present invention provides a fluorescent material with good water resistance, comprising an organic fluorescent glue and a modified fluorescent powder, wherein the modified fluorescent powder is a core-shell structure, wherein the core in the core-shell structure is a mesoporous silica microsphere doped with fluorescent powder, and the shell in the core-shell structure is a compound containing a hydroxyl group, a compound containing an isocyanate group, and polystyrene, wherein the compound containing a hydroxyl group and the compound containing an isocyanate group are coated on the outside of the mesoporous silica microsphere doped with fluorescent powder by polystyrene, and during the preparation process, the hydroxyl group in the compound containing a hydroxyl group and the isocyanate group in the compound containing an isocyanate group react with each other, thereby improving the aging resistance of the fluorescent material. In addition, the fluorescent material has excellent water resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0029] Figure 1 This is a test diagram of the water contact angle of the fluorescent material of Example 3 of the present invention; Figure 2 This is a test diagram of the water contact angle of the fluorescent material of Comparative Example 2 of the present invention; Figure 3 This is a test diagram of the water contact angle of the fluorescent material of Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] The parameters of the raw materials in the following examples and comparative examples are as follows: The polystyrene is Thai Petrochemical polystyrene GP150; The particle size of mesoporous silica microspheres was 90 μm and was purchased from Beijing Zhongke Keyou Technology Co., Ltd.; The phosphor is γ-phase aluminum oxide with a particle size of 20nm and a content of 99.99%; The preparation method of organic fluorescent glue is as follows: Component A of Dow Corning OE-6351 was mixed with 1 / 2 of the mass of component B, and after stirring at 1000 rpm for 20 minutes, the remaining 1 / 2 of the mass of component B was added and stirred for 100 minutes to obtain an organic fluorescent glue, and the mass ratio of component A to component B was 1:1.

[0032] Example 1 S1, 30 g of phosphor, 1 g of mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, after dissolving 2 g of polystyrene in 200 mL of DMF, add the above-mentioned pretreated phosphor, 0.02 g of 1,4-cyclohexanedimethanol, and 0.08 g of 2,4,6-trimethylphenylisocyanate at 15° C., mix, stir at 500 rpm for 30 min until uniform, filter, keep warm at 30° C. for 30 min, dry and remove the solvent, and obtain a modified phosphor; S3. Mix the modified fluorescent powder and the organic fluorescent glue in a mass ratio of 0.7:1, stir at 1000 rpm for 30 min to mix evenly, and obtain a fluorescent material.

[0033] Example 2 S1, 30 g of phosphor, 3 g of mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, after dissolving 2 g of polystyrene in 200 mL of DMF, add the above-mentioned pretreated phosphor, 0.02 g of 1,4-cyclohexanedimethanol, and 0.08 g of 2,4,6-trimethylphenylisocyanate at 15° C., mix, stir at 500 rpm for 30 min until uniform, filter, keep warm at 30° C. for 30 min, dry and remove the solvent, and obtain a modified phosphor; S3. Mix the modified fluorescent powder and the organic fluorescent glue in a mass ratio of 0.7:1, stir at 1000 rpm for 30 min to mix evenly, and obtain a fluorescent material.

[0034] Example 3 S1, 30 g of phosphor, 4 g of mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, after dissolving 2 g of polystyrene in 200 mL of DMF, add the above-mentioned pretreated phosphor, 0.02 g of 1,4-cyclohexanedimethanol, and 0.08 g of 2,4,6-trimethylphenylisocyanate at 15° C., mix, stir at 500 rpm for 30 min until uniform, filter, keep warm at 30° C. for 30 min, dry and remove the solvent, and obtain a modified phosphor; S3. Mix the modified fluorescent powder and the organic fluorescent glue in a mass ratio of 0.7:1, stir at 1000 rpm for 30 min to mix evenly, and obtain a fluorescent material.

[0035] Example 4 S1, 30 g of phosphor, 5 g of mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, after dissolving 2 g of polystyrene in 200 mL of DMF, add the above-mentioned pretreated phosphor, 0.02 g of 1,4-cyclohexanedimethanol, and 0.08 g of 2,4,6-trimethylphenylisocyanate at 15° C., mix, stir at 500 rpm for 30 min until uniform, filter, keep warm at 30° C. for 30 min, dry and remove the solvent, and obtain a modified phosphor; S3. Mix the modified fluorescent powder and the organic fluorescent glue in a mass ratio of 0.7:1, stir at 1000 rpm for 30 min to mix evenly, and obtain a fluorescent material.

[0036] Example 5 S1, 30 g of phosphor, 4 g of mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, after dissolving 2 g of polystyrene in 200 mL of DMF, add the above-mentioned pretreated phosphor, 0.02 g of 1,4-cyclohexanedimethanol, and 0.08 g of 1,6-hexamethylene diisocyanate at 15° C., stir at 500 rpm for 30 min until uniform, filter, keep warm at 30° C. for 30 min, and dry to remove the solvent to obtain a modified phosphor; S3. Mix the modified fluorescent powder and the organic fluorescent glue in a mass ratio of 0.7:1, stir at 1000 rpm for 30 min to mix evenly, and obtain a fluorescent material.

[0037] Example 6 S1, 30 g of phosphor, 4 g of mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, dissolving 2 g of polystyrene in 200 mL of DMF, adding the above-mentioned pretreated phosphor, 0.02 g of 1,4-cyclohexanedimethanol, and 0.08 g of L-lysine triisocyanate at 15° C., stirring at 500 rpm for 30 min until uniform, filtering, keeping warm at 30° C. for 30 min, and drying to remove the solvent to obtain a modified phosphor; S3. Mix the modified fluorescent powder and the organic fluorescent glue in a mass ratio of 0.7:1, stir at 1000 rpm for 30 min to mix evenly, and obtain a fluorescent material.

[0038] Example 7 S1, 30 g of phosphor, 4 g of mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, after dissolving 2 g of polystyrene in 200 mL of DMF, add the above-mentioned pretreated phosphor, 0.1 g of 1,4-cyclohexanedimethanol, and 0.4 g of 1,6-hexamethylene diisocyanate at 15°C, mix, stir at 500 rpm for 30 min until uniform, filter, keep warm at 30°C for 30 min, dry and remove the solvent, and obtain a modified phosphor; S3. Mix the modified fluorescent powder and the organic fluorescent glue in a mass ratio of 0.7:1, stir at 1000 rpm for 30 min to mix evenly, and obtain a fluorescent material.

[0039] Example 8 S1, 30 g of phosphor, 4 g of mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, dissolving 2 g of polystyrene in 200 mL of DMF, adding the above-mentioned pretreated phosphor, 0.2 g of 1,4-cyclohexanedimethanol, and 0.8 g of 1,6-hexamethylene diisocyanate at 15° C., stirring at 500 rpm for 30 min until uniform, filtering, keeping warm at 30° C. for 30 min, and drying to remove the solvent to obtain a modified phosphor; S3. Mix the modified fluorescent powder and the organic fluorescent glue in a mass ratio of 0.7:1, stir at 1000 rpm for 30 min to mix evenly, and obtain a fluorescent material.

[0040] Example 9 S1, 30 g of phosphor, 4 g of mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, after dissolving 2 g of polystyrene in 200 mL of DMF, add the above-mentioned pretreated phosphor, 0.25 g of 1,4-cyclohexanedimethanol, and 0.25 g of 1,6-hexamethylene diisocyanate at 15° C., stir at 500 rpm for 30 min until uniform, filter, keep warm at 30° C. for 30 min, dry and remove the solvent to obtain a modified phosphor; S3. Mix the modified fluorescent powder and the organic fluorescent glue in a mass ratio of 0.7:1, stir at 1000 rpm for 30 min to mix evenly, and obtain a fluorescent material.

[0041] Example 10 S1, 30 g of phosphor, 4 g of mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, after dissolving 2 g of polystyrene in 200 mL of DMF, add the above-mentioned pretreated phosphor, 0.4 g of 1,4-cyclohexanedimethanol, and 0.1 g of 1,6-hexamethylene diisocyanate at 15° C., mix, stir at 500 rpm for 30 min until uniform, filter, keep warm at 30° C. for 30 min, dry and remove the solvent, and obtain a modified phosphor; S3. Mix the modified fluorescent powder and the organic fluorescent glue in a mass ratio of 0.7:1, stir at 1000 rpm for 30 min to mix evenly, and obtain a fluorescent material.

[0042] Comparative Example 1 S1, mixing 30 g of phosphor, 1 g of mesoporous silica microspheres and 450 mL of ethanol, ultrasonically treating at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtering, washing with ethanol, and drying to obtain a modified phosphor; S2. Mix the modified fluorescent powder and the organic fluorescent glue in a mass ratio of 0.7:1, stir at 1000 rpm for 30 min to mix evenly, and obtain a fluorescent material.

[0043] Comparative Example 2 S1, 30 g of phosphor, 1 g of mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, dissolving 2 g of polystyrene in 200 mL of DMF, adding the above-mentioned pretreated phosphor to the mixture at 15° C., stirring at 500 rpm for 30 min until uniform, filtering, keeping warm at 30° C. for 30 min, and drying to remove the solvent to obtain a modified phosphor; S3. Mix the modified fluorescent powder and the organic fluorescent glue in a mass ratio of 0.7:1, stir at 1000 rpm for 30 min to mix evenly, and obtain a fluorescent material.

[0044] The fluorescent materials obtained in Examples 1 to 10 and Comparative Examples 1 to 2 were subjected to an aging resistance test according to the method in GB / T 2689.3-1981 "Simple Linear Unbiased Estimation Method for Life Tests and Accelerated Life Tests (for Weibull Distribution)", and the aging resistance was evaluated by the percentage of the 2000h luminous flux to the initial luminous flux; and the fluorescent materials were coated on a glass substrate, and a water contact angle test was performed to evaluate the water resistance. Figure 1 This is a test diagram of the water contact angle of the fluorescent material of Example 3; Figure 2 This is a water contact angle test diagram of the fluorescent material of Comparative Example 2; Figure 3 This is a water contact angle test diagram of the fluorescent material of Comparative Example 1; the test results are recorded in Table 1.

[0045] Table 1 Aging resistance and water resistance of fluorescent materials

[0046] It can be seen from Table 1 that the fluorescent material provided by the present invention has good aging resistance and water resistance.

[0047] Compared with Comparative Examples 1-2, the modified phosphor in Examples 1-10 is a core-shell structure, the core in the core-shell structure is a mesoporous silica microsphere doped with phosphor, and the shell in the core-shell structure is a compound containing a hydroxyl group, a compound containing an isocyanate group, and polystyrene. The percentage of 2000h luminous flux to initial luminous flux and the water contact angle of the fluorescent material obtained in Examples 1-10 are higher than those in Comparative Examples 1-2, indicating that the core in the core-shell structure is a mesoporous silica microsphere doped with phosphor, and the shell in the core-shell structure is a compound containing a hydroxyl group, a compound containing an isocyanate group, and polystyrene, which can improve the aging resistance and water resistance of the fluorescent material.

[0048] The percentage of 2000h luminous flux to initial luminous flux and water contact angle of the fluorescent materials obtained in Examples 2-3 are higher than those in Example 1 and Example 4, indicating that the raw materials of the core are phosphor and mesoporous silica microspheres in a mass ratio of 30:3-4, which can further improve the aging resistance and water resistance of the fluorescent material.

[0049] The percentage of the 2000h luminous flux to the initial luminous flux and the water contact angle of the fluorescent material obtained in Example 5 are higher than those in Example 3 and Example 6, indicating that the compound containing an isocyanate group is a compound containing two isocyanate groups, which can further improve the aging resistance and water resistance of the fluorescent material.

[0050] The percentage of the 2000h luminous flux of the fluorescent material obtained in Example 7 to the initial luminous flux and the water contact angle are higher than those in Example 5 and Example 8, indicating that the mass ratio of the hydroxyl group-containing compound and the isocyanate group-containing compound to the mass ratio of polystyrene is 0.5:2, which can further improve the aging resistance and water resistance of the fluorescent material.

[0051] The percentage of the 2000h luminous flux of the fluorescent material obtained in Example 9 to the initial luminous flux and the water contact angle are higher than those in Example 7 and Example 10, indicating that the mass ratio of the compound containing a hydroxyl group to the compound containing an isocyanate group is 1:1, which can further improve the aging resistance and water resistance of the fluorescent material.

[0052] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A fluorescent material with good water resistance, characterized in that: It comprises organic fluorescent glue and modified fluorescent powder, wherein the modified fluorescent powder is a core-shell structure, the core of the core-shell structure is a mesoporous silica microsphere doped with fluorescent powder, and the shell of the core-shell structure is a compound containing hydroxyl group, a compound containing isocyanate group and polystyrene.

2. The fluorescent material with good water resistance according to claim 1, characterized in that: The mass ratio of the compound containing a hydroxyl group and the compound containing an isocyanate group to the polystyrene is 0.1 to 1:

2.

3. The fluorescent material with good water resistance according to claim 2, characterized in that: The mass ratio of the compound containing a hydroxyl group to the compound containing an isocyanate group is 0.1-0.4:0.4-0.

1.

4. The fluorescent material with good water resistance according to claim 3, characterized in that: The isocyanate group-containing compound is a compound containing two or more isocyanate groups.

5. The fluorescent material with good water resistance according to claim 4, characterized in that: The isocyanate group-containing compound is a compound containing two isocyanate groups.

6. The fluorescent material with good water resistance according to claim 1, characterized in that: The hydroxyl group-containing compound is 1,4-cyclohexanedimethanol.

7. The fluorescent material with good water resistance according to claim 1, characterized in that: The mass ratio of the raw material of the core to the raw material of the shell is 30-35:2-3.

8. The fluorescent material with good water resistance according to claim 1, characterized in that: The raw materials of the core include phosphor and mesoporous silica microspheres in a mass ratio of 30:3-4.

9. The method for preparing a fluorescent material with good water resistance according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, mixing the phosphor, mesoporous silica microspheres and solvent uniformly, filtering, washing and drying to obtain pretreated phosphor; S2, uniformly mixing the pretreated phosphor, the compound containing a hydroxyl group, the compound containing an isocyanate group, polystyrene and a solvent, filtering and drying to obtain a modified phosphor; S3, mixing the modified fluorescent powder and the organic fluorescent glue evenly to obtain a fluorescent material.

10. The method for preparing a fluorescent material with good water resistance according to claim 9, characterized in that: The solvent in S2 is N,N-dimethylformamide, and the mixing temperature is 15-20° C.; before drying, the temperature is raised to 25-30° C. and kept warm for 20-40 minutes.