Method for improving enzymolysis efficiency of high-solid-content lignocellulose

By adding aqueous ethanol solution, PEG8000, NaOH and Tween 80 during the pretreatment and enzymatic stages, the problem of low enzymatic lignocellulose at high solids content is solved, and efficient enzymatic lysis and high concentration sugar product generation are achieved. Improves the efficiency of biomass conversion.

CN119020437APending Publication Date: 2024-11-26SOUTH CHINA AGRICULTURAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411036807.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Under high solid content conditions, lignocellulose enzymatic efficiency is low, and cellulases are prone to inactivate, making it difficult to mix effectively, affecting the efficiency of biomass conversion.

Method used

In the pretreatment and enzymatic stage, add aqueous ethanol solution, PEG8000, NaOH and surfactant Tween 80, and after pretreatment, add buffer solution and cellulase to control the solid-liquid ratio to 10-15% to reduce the cellulase Ineffective adsorption and improve mixing uniformity.

Benefits of technology

It significantly improves the enzymatic efficiency of high solid content lignocellulose, produces high concentrations of glucose and xylose, reduces the difficulty of the mass transfer process, and improves the high-value utilization of lignocellulose.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004971310280000041
    Figure BDA0004971310280000041
  • Figure BDA0004971310280000051
    Figure BDA0004971310280000051
  • Figure BDA0004971310280000053
    Figure BDA0004971310280000053
Patent Text Reader

Abstract

The invention discloses a method for improving the enzymolysis efficiency of high-solid-content lignocellulose. According to the method, the surfactant is added in the pretreatment stage and the enzymolysis stage, so that the enzymolysis efficiency of the lignocellulose can be improved under the condition that the solid-to-liquid ratio is 10-15%, meanwhile, high-concentration glucose and xylose are generated, and a synergistic interaction effect is achieved. According to the method, the ineffective adsorption of the lignocellulose to the cellulase under the high-solid condition is reduced, the difficulty of the mass transfer process and effective uniform mixing is reduced, and the method has a wide application prospect in the aspect of high-value utilization of the lignocellulose.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomass conversion and utilization, and in particular to a method for improving the enzymatic hydrolysis efficiency of high-solid-content lignocellulose. Background Art

[0002] Enzymatic hydrolysis is a key step in converting lignocellulosic biomass into ethanol and other value-added products. Although many pretreatment technologies can break the physical barrier of lignocellulose and improve the efficiency of enzymatic hydrolysis, some lignin still remains in the sample after pretreatment, which will inactivate cellulase through ineffective adsorption or reduce the accessibility of enzymes to cellulose through steric hindrance. Studies have found that adding surfactants during enzymatic hydrolysis can significantly improve the conversion rate of lignocellulose enzymatic hydrolysis, reduce the ineffective adsorption of lignin to enzymes, and thus reduce the amount of cellulase used.

[0003] Increasing the solid content is also a way to improve the conversion of lignocellulosic biomass. However, enzymatic hydrolysis requires the participation of water molecules. Too high a solid content will absorb free water molecules, which mostly exist in a bound form. The reduction of free water will increase the energy required for mixing the raw materials during the reaction process, limiting the adsorption of cellulase and substrate, and increasing the difficulty of mass transfer and effective mixing. Therefore, it is crucial to find a method that can improve the efficiency of enzymatic hydrolysis under high solid conditions. Summary of the invention

[0004] In order to overcome the above defects and shortcomings in the prior art, the present invention provides a method for improving the enzymatic hydrolysis efficiency of high-solid content lignocellulose.

[0005] The first object of the present invention is to provide a method for improving the enzymatic hydrolysis efficiency of high-solid content lignocellulose.

[0006] Therefore, the present invention claims the following:

[0007] A method for improving the enzymatic hydrolysis efficiency of high-solid content lignocellulose comprises the following steps:

[0008] S1. Adding ethanol aqueous solution, PEG8000 and NaOH to the lignocellulose raw material for pretreatment to obtain pretreated lignocellulose;

[0009] S2. Adding a buffer solution, Tween 80 and cellulase to the pretreated lignocellulose in step S1, mixing well and performing enzymolysis;

[0010] The high solid content lignocellulose is a pretreated lignocellulose, and the ratio of the absolute dry mass to the total volume of the cellulase and the buffer solution is (1-1.6) g:10 mL.

[0011] Preferably, in step S1, the ratio of the absolute dry mass of the lignocellulosic raw material to ethanol, PEG8000 and NaOH is 1 g: (5.8-6.2) mL: (43-47) mg: (0.4-0.8) g.

[0012] More preferably, the ratio of the absolute dry mass of the lignocellulosic raw material to ethanol, PEG8000 and NaOH is 1 g: 6 mL: 45 mg: 0.6 g.

[0013] Preferably, in step S1, the pretreatment temperature is 155-165°C.

[0014] More preferably, the pretreatment temperature is 160°C.

[0015] Preferably, in step S1, the pretreatment time is 8 to 12 minutes.

[0016] More preferably, the pretreatment time is 10 min.

[0017] Preferably, in step S2, the ratio of the absolute dry mass of the pretreated lignocellulose to Tween 80 is 1 g: (43-47) mg.

[0018] More preferably, the ratio of the absolute dry mass of the pretreated lignocellulose to Tween 80 is 1 g:45 mg.

[0019] Preferably, in step S2, the ratio of the absolute dry weight of the pretreated lignocellulose to the cellulase is 1 g: (8-12) FPU.

[0020] More preferably, the ratio of the absolute dry weight of the pretreated lignocellulose to the cellulase is 1 g:10 FPU.

[0021] More preferably, the cellulase is Cellulase II.

[0022] Preferably, in step S2, the buffer solution is an acetic acid-sodium acetate buffer solution.

[0023] Preferably, in step S2, the temperature of the enzymatic hydrolysis is 45-55°C.

[0024] More preferably, the temperature of the enzymatic hydrolysis is 50°C.

[0025] Preferably, the ratio of the absolute dry mass of the high-solid content lignocellulose to the total volume of the cellulase and the buffer solution is 1 g:10 mL, and the enzymatic hydrolysis time is 12 to 96 hours.

[0026] More preferably, the enzymatic hydrolysis time is 96 h.

[0027] Preferably, the ratio of the absolute dry mass of the high-solid content lignocellulose to the total volume of the cellulase and the buffer solution is 1.6 g:10 mL, and the enzymatic hydrolysis time is 48 to 144 h.

[0028] More preferably, the enzymatic hydrolysis time is 96 to 120 hours.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The present invention discloses a method for improving the enzymatic hydrolysis efficiency of high-solid content lignocellulose. The present invention can improve the enzymatic hydrolysis efficiency of lignocellulose under the condition of a solid-liquid ratio of 10 to 15% by adding a surfactant in both the pretreatment stage and the enzymatic hydrolysis stage, and simultaneously produce high concentrations of glucose and xylose, thereby playing a synergistic effect. The method reduces the ineffective adsorption of lignocellulose to cellulase under high-solid conditions, reduces the difficulty of mass transfer process and effective mixing, and has broad application prospects in the high-value utilization of lignocellulose. DETAILED DESCRIPTION

[0031] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0032] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0033] The bagasse raw material used is air-dried and pulverized, and its component contents are 41.94% cellulose, 22.34% hemicellulose, and 22.35% lignin.

[0034] The cellulase was Celly II enzyme purchased from Novozymes (China) Biotechnology Co., Ltd.

[0035] Preparation of 0.05 mol / L acetic acid-sodium acetate buffer solution: weigh 4.1 g of anhydrous sodium acetate and dissolve it in 500 mL of distilled water and dilute to obtain a sodium acetate solution; weigh 1.5 g of acetic acid and dissolve it in 250 mL of distilled water and dilute to obtain an acetic acid solution; then take 300 mL of the sodium acetate solution and mix it with 200 mL of the acetic acid solution and dilute to volume.

[0036] Glucose in the enzymatic hydrolysate was directly determined by high performance liquid chromatography.

[0037] The use of bagasse is for exemplary purposes only, and lignocellulose from other sources may also be used instead of bagasse. Raw materials that may replace bagasse include, but are not limited to, poplar, eucalyptus, corn stalks, wheat stalks, corn cobs, and the like.

[0038] Example 1 A method for improving the efficiency of enzymatic hydrolysis of high solid content lignocellulose

[0039] S1. Add 60% (v / v) ethanol aqueous solution to the bagasse raw material at an absolute dry mass volume ratio of 1g:10mL, add 45mg / g 绝干质量的甘蔗渣原料 Polyethylene glycol 8000, then add 10% NaOH (w / v 60%乙醇水溶液 ) were mixed in a reaction kettle, and heat-treated at 300 rpm and 160° C. for 10 min. After vacuum filtration, polyethylene glycol 8000-assisted NaOH-enhanced ethanol pretreated bagasse was obtained. After vacuum filtration, the moisture content of the pretreated bagasse was about 70% (w / w);

[0040] S2. Add 0.05 mol / L acetic acid-sodium acetate buffer solution to the pretreated bagasse obtained in step S1, and add 10 FPU / g of cellulase 绝干质量的预处理甘蔗渣 , so that the solid-liquid ratio reaches 10% (absolute dry mass of pretreated bagasse / (volume of cellulase+volume of acetic acid-sodium acetate buffer solution)). In addition, 45 mg / g 绝干质量的预处理甘蔗渣 Tween 80 was added and mixed evenly, then placed in a constant temperature shaker for enzymatic hydrolysis. The shaking speed was set to 150 rpm and the temperature was set to 50 °C. When the enzymatic hydrolysis time reached 12 h, 24 h, 48 h, 72 h and 96 h, 1 mL of supernatant was taken to detect the glucose content obtained by hydrolysis.

[0041] Example 2 A method for improving the efficiency of enzymatic hydrolysis of high solid content lignocellulose

[0042] The method of Example 1 was followed, except that the solid-liquid ratio in step S2 reached 16% (absolute dry mass of pretreated bagasse / (volume of cellulase+volume of acetic acid-sodium acetate buffer solution)). When the enzymolysis time reached 48 h, 72 h, 96 h, 120 h and 144 h, 1 mL of supernatant was taken to detect the glucose and xylose content obtained by hydrolysis.

[0043] Comparative Example 1

[0044] The method of Example 1 is followed, except that in step S1, the amount of polyethylene glycol 8000 added is 0; and in step S2, the amount of Tween 80 added is 0.

[0045] Comparative Example 2

[0046] The method of Example 1 is followed, except that the amount of Tween 80 added in step S2 is 0.

[0047] Comparative Example 3

[0048] The method of Example 1 is followed, except that in step S1, the amount of polyethylene glycol 8000 added is 0.

[0049] Comparative Example 4

[0050] The method of Example 2 is followed, except that in step S1, the amount of polyethylene glycol 8000 added is 0; and in step S2, the amount of Tween 80 added is 0.

[0051] Comparative Example 5

[0052] The method of Example 2 is followed, except that the amount of Tween 80 added in step S2 is 0.

[0053] Comparative Example 6

[0054] The method of Example 2 is followed, except that in step S1, the amount of polyethylene glycol 8000 added is 0.

[0055] Performance Test 1

[0056] The glucose concentration in the enzymolysis solution of Example 1 and Comparative Examples 1 to 3 during enzymolysis for 0 to 96 hours was determined by high performance liquid chromatography. The specific results are shown in Tables 1 and 2.

[0057] Table 1 Glucose concentration in the enzymatic hydrolysate from 0 to 96 h (g / L)

[0058]

[0059]

[0060] The glucose concentration growth rate (Table 2) was calculated based on the glucose concentration in Table 1, and the calculation formula is shown in Formula (I):

[0061]

[0062] Table 2 Growth rate of glucose concentration in the enzymatic hydrolysate from 0 to 96 h (%)

[0063]

[0064] As shown in Table 1 and Table 2, when the solid-liquid ratio is 10%, the glucose concentration of Example 1 is significantly improved compared with that of Comparative Example 1 during the enzymatic hydrolysis from 0 to 96 hours. At 12 hours, the glucose concentration of Example 1 far exceeds that of Comparative Example 1, and the glucose concentration growth rate is as high as 143.12%. The peak of the glucose concentration growth rate occurs at 24 hours. Although it partially decreases at 48 hours and 72 hours, the glucose concentration growth rate is still maintained at 112.66% at 96 hours. The data show that Example 1 is significantly improved compared with Comparative Example 1.

[0065] At the same time, the glucose concentration of Example 1 is also improved compared with Comparative Example 2, and the glucose concentration growth rate shows a trend of first increasing and then decreasing. The peak of the glucose concentration growth rate appears at 48h, reaching 49.18%. Although it decreases later, the glucose concentration growth rate remains at 20.62% at 96h, which is improved compared with Comparative Example 2.

[0066] By comparing Example 1 with Comparative Example 3, it can be observed that during the enzymatic hydrolysis period, the glucose concentration still retains a certain growth rate. By comparing Example 1 with Comparative Examples 1 to 3, it can be observed that adding surfactants in both the pretreatment stage and the enzymatic hydrolysis stage has a certain synergistic effect, which can significantly improve the enzymatic hydrolysis efficiency.

[0067] Test performance 2

[0068] The concentrations of glucose and xylose in the enzymatic fermentation broth of Example 2 and Comparative Examples 4 to 6 at 0 to 144 h of enzymatic hydrolysis were determined by high performance liquid chromatography. The specific results are shown in Table 3.

[0069] Table 3 Glucose and xylose concentrations in the enzymatic hydrolysate from 0 to 144 h (g / L)

[0070]

[0071] The growth rates of glucose and xylose concentrations were calculated according to the glucose concentrations in Table 3 (Table 4), wherein the growth rate of glucose concentration is shown in formula (I), and the growth rate of xylose concentration is shown in formula (II):

[0072]

[0073] Table 4 Growth rate of glucose and xylose concentration in the enzymatic hydrolysate from 0 to 144 h (%)

[0074]

[0075] As shown in Tables 3 and 4, when the solid-liquid ratio is 16%, the concentration of glucose and xylose in Example 2 is significantly improved compared with Comparative Examples 4 to 6 during 0 to 144 hours of enzymolysis. Example 2 reaches the highest fermentable sugar (glucose and xylose) concentration of 129.96 g / L at 120 hours, and the xylose concentration growth rate at 120 hours is 18.29% (relative to Comparative Example 4), 5.42% (relative to Comparative Example 5) and 13.91% (relative to Comparative Example 6). The highest fermentable sugar (glucose and xylose) concentration of Comparative Example 4 is 115.21 g / L, which occurs at 144 hours of enzymolysis. Compared with Comparative Example 4, not only does Example 2 have the highest concentration 24 hours earlier than Comparative Example 4, but the highest concentration is also improved. The highest fermentable sugar (glucose and xylose) concentration of Comparative Example 5 is 124.14 g / L, which occurs at 120 hours of enzymolysis. The highest concentration of Example 2 is also increased compared with Comparative Example 5. It can be seen that adding surfactants in both the pretreatment and enzymolysis stages can significantly improve the enzymolysis efficiency.

[0076] Combined with Tables 1 to 4, the addition of surfactants in both the pretreatment and enzymolysis stages improves the enzymolysis efficiency at a higher solid load. It can be seen that the method according to the present invention can effectively improve the enzymolysis efficiency and increase the yield of glucose and xylose.

[0077] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for improving the enzymatic hydrolysis efficiency of high-solid content lignocellulose, It is characterized in that The following steps are involved: S1. Adding ethanol aqueous solution, PEG8000 and NaOH to the lignocellulose raw material for pretreatment to obtain pretreated lignocellulose; S2. Adding a buffer solution, Tween 80 and cellulase to the pretreated lignocellulose in step S1, mixing well and performing enzymolysis; The high solid content lignocellulose is a pretreated lignocellulose, and the ratio of the absolute dry mass to the total volume of the cellulase and the buffer solution is (1-1.6) g:10 mL.

2. The method according to claim 1, It is characterized in that In step S1, the ratio of the absolute dry mass of the lignocellulose raw material to ethanol, PEG8000 and NaOH is 1 g: (5.8-6.2) mL: (43-47) mg: (0.4-0.8) g.

3. The method according to claim 1, It is characterized in that In step S1, the pretreatment temperature is 155-165°C.

4. The method according to claim 1, It is characterized in that In step S1, the pretreatment time is 8 to 12 minutes.

5. The method according to claim 1, It is characterized in that In step S2, the ratio of the absolute dry weight of the pretreated lignocellulose to Tween 80 is 1 g: (43-47) mg.

6. The method according to claim 1, It is characterized in that In step S2, the ratio of the absolute dry weight of the pretreated lignocellulose to the cellulase is 1 g: (8-12) FPU.

7. The method according to claim 1, It is characterized in that In step S2, the buffer solution is an acetic acid-sodium acetate buffer solution.

8. The method according to claim 1, It is characterized in that In step S2, the temperature of the enzymatic hydrolysis is 45-55°C.

9. The method according to claim 1, It is characterized in that The ratio of the absolute dry mass of the high solid content lignocellulose to the total volume of the cellulase and the buffer solution is 1 g:10 mL, and the enzymolysis time is 12 to 96 hours.

10. The method according to claim 1, It is characterized in that The ratio of the absolute dry mass of the high solid content lignocellulose to the total volume of the cellulase and the buffer solution is 1.6 g:10 mL, and the enzymolysis time is 48 to 144 hours.