Heat treatment process technology preparation method for replacing offline normalizing with online normalizing for high-pressure alloy boiler pipe

By replacing offline normalizing heat treatment process, the problem of 15CrMoG steel pipe not meeting the performance standards after traditional heat treatment is solved, and the good strength, oxidation resistance and corrosion resistance of high-pressure alloy boiler pipes are achieved, and production costs are reduced. Energy consumption.

CN119020559APending Publication Date: 2024-11-26BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411083874.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

After traditional normalization + tempering heat treatment, the structure and performance of 15CrMoG steel pipes are difficult to meet the standard requirements, and the amount of alloy added increases production costs.

Method used

Online normalization is used instead of offline normalization heat treatment technology, and the phase change of grain structure is improved and production costs are reduced by controlling the heating and tempering temperature.

Benefits of technology

The uniform refinement of the 15CrMoG steel pipe is achieved and the good mechanical properties are good, which reduces production costs and energy consumption and improves process control stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020559A_ABST
    Figure CN119020559A_ABST
Patent Text Reader

Abstract

The invention discloses a heat treatment process technology preparation method for replacing offline normalizing with online normalizing for a high-pressure alloy boiler pipe. The main process steps and process parameters are as follows: 1) blank inspection; 2) heating the tube blank; 3) a continuous rolling process; (4) an on-line normalizing and off-line tempering heat treatment process is carried out, the finish rolling temperature is increased and controlled to be 880 DEG C, then tempering is carried out, the tempering temperature is 690 + / -10 DEG C, and the tempering time is 80 min; the invention further discloses the chemical components of the high-pressure alloy boiler pipe according to the weight percentage. The prepared high-pressure alloy boiler pipe has good obdurability, high-temperature oxidation resistance, heat resistance and good sulfur and hydrogen corrosion resistance, and the alloy steel manufacturing method is low in production cost and short in production period. The production process is stable to control, and the production cost and energy consumption are greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alloy boiler tubes for containers, and in particular relates to a preparation method of a high-pressure alloy boiler tube by online normalizing instead of offline normalizing heat treatment process technology. Background Art

[0002] 15CrMoG belongs to alloy structural steel, also known as chromium-molybdenum steel. Because of the high Cr and Mo content in the steel, it has good resistance to hydrogen and sulfur corrosion and good high-temperature oxidation resistance. It also has good process performance and welding performance. It is often used in pipe fittings and equipment in industries such as petroleum, heat, steam, and pressure cookers. Boiler pipe 15CrMoG often has a structure or performance that cannot meet the standard requirements of GB / T5310-2017 after normalizing + tempering heat treatment. In response to the above problems, different heat treatment processes are debugged, and online normalizing of steel pipes is used instead of offline normalizing heat treatment process, which greatly improves the phase transformation and refinement effect of grain structure. Finally, the heat treatment structure of 15CrMoG steel pipe is uniformly refined and the mechanical properties are good. More importantly, the production process control is stable, and the production cost and energy consumption are greatly reduced.

[0003] Li Jinrong et al. (Li Jinrong et al., 15CrMoG Large Diameter High Pressure Boiler Tube Heat Treatment Process Practice, Modern Metallurgy, Issue 8, 2020) developed a 15CrMoG high pressure boiler with a high amount of Mo alloy added, which increased production costs. After heat treatment at a normalizing temperature of 920-950℃ and a tempering temperature of 680-720℃, the yield strength is 355MPa and the tensile strength is 452MPa, which can obtain a good match of strength and toughness, but the strength surplus is not large.

[0004] Feng Danzhu et al. (Feng Danzhu et al., Influence of Heat Treatment Process on the Microstructure and Properties of 15CrMo Alloy Structural Steel, Anshan Iron and Steel Technology, Issue 1, 2024) developed the composition mass percentage as follows: C 0.15%, Si 0.27%, Mn 0.55%, Cr0.85%, Mo 0.42%, and the balance is iron. After normalizing at 900℃ for 120min and tempering at 650℃ for 120min, the tensile strength is 516MPa, the yield strength is 367MPa, and the elongation is 25.0%. However, the amount of Mo alloy added is relatively high, which increases the production cost.

[0005] Hua Longlong et al. (Hualonglong et al., Research on Microstructure and Mechanical Properties of 15CrMo Steel Pipe Neck Forming, Hot Working Technology, Issue 12, 2023) developed the composition mass percentage as follows: C 0.12-0.18% Si0.17-0.37% Mn 0.40-0.70% P 0.0035% S 0.0035% Cr 0.80-1.10% Mo0.40-0.55% Ni 0.03%, but the amount of Ni alloy added is relatively high, which increases the production cost. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a high-pressure alloy boiler tube by online normalizing instead of offline normalizing heat treatment process technology, and the high-pressure alloy boiler tube has good toughness, high-temperature oxidation resistance, thermal strength and good resistance to sulfur and hydrogen corrosion, and has a low production cost and a short production cycle. The production process control is stable, and the production cost and energy consumption are greatly reduced.

[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0008] The present invention discloses a method for preparing a high-pressure alloy boiler tube by online normalizing instead of offline normalizing heat treatment process technology, and the main process steps and process parameters are as follows:

[0009] 1) Billet inspection;

[0010] 2) Tube heating

[0011] Continuously check the temperature of each section such as preheating section, heating section, soaking section, etc. to ensure thorough and uniform heating without over-burning. The temperature of each section of the ring furnace is controlled. The temperature of heating zone 1 is 1045-1065℃, the temperature of heating zone 2 is 1245-1265℃, and the soaking zone is 1240-1260℃;

[0012] 3) Continuous rolling process

[0013] Carry out continuous rolling and piercing process; the temperature after piercing is 1190℃-1210℃; the final rolling temperature is 830℃-880℃; the cooling water of the steel pipe is controlled, the continuous rolling mill is water-controlled rolling, and the dephosphorization water pressure is 9-10MPa;

[0014] 4) Normalizing + tempering heat treatment

[0015] The steel pipe samples after rolling and cooling are subjected to normalizing and tempering heat treatment; two different heat treatment processes are adopted: one process is that the steel pipe is subjected to hot rolling with a final rolling temperature of 830-840℃, a normalizing temperature of 940±10℃, a normalizing time of 80min, a tempering temperature of 690±10℃, and a tempering time of 80min; the other process is an online normalizing + offline tempering heat treatment process, which increases the final rolling temperature compared to the first heat treatment scheme, controls the final rolling temperature to 880℃, and then performs tempering, with a tempering temperature of 690±10℃ and a tempering time of 80min;

[0016] The chemical composition of the high-pressure alloy boiler tube is C: 0.12-0.14%, Si: 0.45-0.50%, Mn: 0.70-0.90%, P: ≤0.016%, S≤0.005%, Mo: 0.35-0.40%, Ti: 0.06-0.08%, Cr: 1.50-1.70%, and the balance is Fe and unavoidable impurities.

[0017] Furthermore, the above 1) specifically includes: there shall be no visible scars, cracks, sand holes, inclusions, pores and pinhole defects on the surface of the tube blank; batching principle: steel pipes shall be inspected and accepted in batches, and each batch shall consist of steel pipes of the same brand, same furnace number, same specification and same heat treatment system.

[0018] Furthermore, in the above 2), the discharging rhythm is controlled to be 54 pieces / second.

[0019] Furthermore, the continuous rolling piercing process includes: the piercing mill roll spacing is 136mm, the guide plate spacing is 156mm, the head position is 95-105mm, the rotation speed is 330-630rpm, the front pressing rate is 5.1%, the speed increase ratio is 1.9, the ovality is 1.15, and the outlet speed is 0.6m / s.

[0020] Furthermore, the chemical composition of the high-pressure alloy boiler tube is C: 0.12%, Si: 0.45%, Mn: 0.70%, P: 0.015%, S 0.005%, Mo: 0.35%, Ti: 0.06%, Cr: 1.50%, and the balance is Fe and unavoidable impurities.

[0021] Furthermore, the chemical composition of the high-pressure alloy boiler tube is C: 0.13%, Si: 0.48%, Mn: 0.80%, P: 0.007%, S 0.003%, Mo: 0.38%, Ti: 0.07%, Cr: 1.64%, and the balance is Fe and unavoidable impurities.

[0022] Furthermore, the chemical composition of the high-pressure alloy boiler tube is C: 0.14%, Si: 0.50%, Mn: 0.90%, P: 0.015%, S 0.005%, Mo: 0.40%, Ti: 0.08%, Cr: 1.70%, and the balance is Fe and unavoidable impurities.

[0023] Compared with the prior art, the beneficial technical effects of the present invention are:

[0024] The present invention provides a 15CrMoG high-pressure alloy boiler tube online normalizing instead of offline normalizing heat treatment process technology preparation method, in particular, the alloy steel manufacturing method has good toughness, high temperature oxidation resistance, thermal strength and good resistance to sulfur and hydrogen corrosion, short production cycle, and greatly reduced production cost and energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The present invention will be further described below in conjunction with the accompanying drawings.

[0026] Figure 1 The metallographic structure of Example 1 of the present invention;

[0027] Figure 2 This is the metallographic structure of Example 2 of the present invention. DETAILED DESCRIPTION

[0028] The present invention is described in more detail below with examples. These examples are merely descriptions of the best mode for carrying out the present invention and are not intended to limit the scope of the present invention in any way.

[0029] Example 1

[0030] The surface of the tube shall not have visually visible defects such as scars, cracks, sand holes, inclusions, pores and pinholes. Continuously check the temperature of each section such as the preheating section, heating section, and soaking section to ensure thorough and uniform heating without overburning, and control the temperature of each section of the ring furnace. The temperature of the heating zone 1 is 1045℃, the temperature of the heating zone 2 is 1245℃, and the soaking zone is 1240℃. Carry out continuous rolling piercing process, the roller spacing of the piercing mill is 136mm, the guide plate spacing is 156mm, the head position is 95mm, the speed is 330rpm, the front pressure reduction rate is 5.1%, the speed increase ratio is 1.9, the ovality is 1.15, and the exit speed is 0.6m / s. The temperature after piercing is 1190℃. The final rolling temperature is 830℃. The cooling water of the steel pipe is controlled, the continuous rolling mill is water-controlled rolling, and the dephosphorization water pressure is 9MPa. The steel pipe samples after rolling and cooling were subjected to normalizing and tempering heat treatment experiments, with offline normalizing + offline tempering heat treatment processes, the steel pipe final rolling temperature was 830°C, the offline normalizing temperature was 940±10°C, the normalizing time was 80min, the tempering temperature was 690±10°C, and the tempering time was 80min.

[0031] Example 2

[0032] The surface of the tube shall not have visually visible scars, cracks, sand holes, inclusions, pores and pinholes. Continuously check the temperature of each section such as the preheating section, heating section, and soaking section to ensure thorough and uniform heating without overheating, and control the temperature of each section of the ring furnace. The temperature of the heating zone 1 is 1055℃, the temperature of the heating zone 2 is 1255℃, and the soaking zone is 1250℃. Carry out continuous rolling piercing process, the roller spacing of the piercing mill is 136mm, the guide plate spacing is 156mm, the head position is 95mm, the speed is 430rpm, the front pressure reduction rate is 5.1%, the speed increase ratio is 1.9, the ovality is 1.15, and the exit speed is 0.6m / s. The temperature after piercing is 1200℃. The final rolling temperature is 880℃. The cooling water of the steel pipe is controlled, the continuous rolling mill is water-controlled rolling, and the dephosphorization water pressure is 9.5MPa. The steel pipe samples after rolling and cooling were subjected to normalizing and tempering heat treatment experiments. The online normalizing + offline tempering heat treatment process increased the final rolling temperature of the steel pipe to 880°C, and then offline tempering was performed. The tempering temperature was 690±10°C and the tempering time was 80 minutes. By increasing the final rolling temperature, it is also called online normalizing, which directly replaces offline normalizing, saving processes, shortening the production cycle, and greatly reducing production costs and energy consumption.

[0033] Example 3

[0034] The surface of the tube shall not have visually visible defects such as scars, cracks, sand holes, inclusions, pores and pinholes. Continuously check the temperature of each section such as the preheating section, heating section, and soaking section to ensure thorough and uniform heating without overburning, and control the temperature of each section of the ring furnace. The temperature of the heating zone 1 is 1065℃, the temperature of the heating zone 2 is 1265℃, and the soaking zone is 1260℃. Carry out continuous rolling piercing process, the roller spacing of the piercing mill is 136mm, the guide plate spacing is 156mm, the head position is 95mm, the speed is 630rpm, the front pressure reduction rate is 5.1%, the speed increase ratio is 1.9, the ovality is 1.15, and the exit speed is 0.6m / s. The temperature after piercing is 1210℃. The final rolling temperature is 840℃. The cooling water of the steel pipe is controlled, the continuous rolling mill is water-controlled rolling, and the dephosphorization water pressure is 10MPa. The steel pipe samples after rolling and cooling were subjected to normalizing and tempering heat treatment experiments, with offline normalizing + offline tempering heat treatment processes. The steel pipe final rolling temperature was 840°C, the normalizing temperature was 940±10°C, the normalizing time was 80min, the tempering temperature was 690±10°C, and the tempering time was 80min.

[0035] Table 1 Chemical composition of Examples 1 to 3 of the present invention (wt%)

[0036] Example C Si Mn P S Mo Cr Ti T 0.12 0.45 0.70 0.015 0.005 0.35 1.50 0.06 2 0.13 0.48 0.80 0.007 0.003 0.38 1.64 0.07 3 0.14 0.50 0.90 0.015 0.005 0.40 1.70 0.08

[0037] Table 2 Mechanical properties of heat-treated steel pipes of Examples 1 to 3 of the present invention

[0038]

[0039] It can be seen from the data in Table 2 that the preparation method of the high-pressure alloy boiler tube provided by the present invention is a heat treatment process technology for replacing the off-line normalizing with the online normalizing. The mechanical properties and process properties meet the yield strength of 440-640MPa, the tensile strength ≥295MPa, the elongation A ≥21%, and have a good hardness value. The mechanical properties under the two test schemes are slightly different. The tensile strength and yield strength of the off-line heat treatment method are lower than those of the online normalizing heat treatment scheme, and the elongation is higher. In addition, the metallographic structure of Example 2 is finer than that of Example 1. From the results of the above embodiments, it can be seen that the high-pressure alloy boiler tube of the present invention has good toughness, high temperature oxidation resistance, heat strength and good resistance to sulfur and hydrogen corrosion.

[0040] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A high-pressure alloy boiler tube online normalizing instead of offline normalizing heat treatment process technology preparation method, characterized in that: The main process steps and process parameters are as follows: 1) Billet inspection; 2) Tube heating Continuously check the temperature of each section such as preheating section, heating section, soaking section, etc. to ensure thorough and uniform heating without over-burning. The temperature of each section of the ring furnace is controlled. The temperature of heating zone 1 is 1045-1065℃, the temperature of heating zone 2 is 1245-1265℃, and the soaking zone is 1240-1260℃; 3) Continuous rolling process Carry out continuous rolling and piercing process; the temperature after piercing is 1190℃-1210℃; the final rolling temperature is 830℃-880℃; the cooling water of the steel pipe is controlled, the continuous rolling mill is water-controlled rolling, and the dephosphorization water pressure is 9-10MPa; 4) Normalizing + tempering heat treatment The steel pipe samples after rolling and cooling are subjected to normalizing and tempering heat treatment; two different heat treatment processes are adopted: one process is that the steel pipe is subjected to hot rolling with a final rolling temperature of 830-840℃, a normalizing temperature of 940±10℃, a normalizing time of 80min, a tempering temperature of 690±10℃, and a tempering time of 80min; the other process is an online normalizing + offline tempering heat treatment process, which increases the final rolling temperature compared to the first heat treatment scheme, controls the final rolling temperature to 880℃, and then performs tempering, with a tempering temperature of 690±10℃ and a tempering time of 80min; The chemical composition of the high-pressure alloy boiler tube is C: 0.12-0.14%, Si: 0.45-0.50%, Mn: 0.70-0.90%, P: ≤0.016%, S≤0.005%, Mo: 0.35-0.40%, Ti: 0.06-0.08%, Cr: 1.50-1.70%, and the balance is Fe and unavoidable impurities.

2. The method for preparing a high-pressure alloy boiler tube by online normalizing instead of offline normalizing heat treatment process technology according to claim 1, characterized in that: The above 1) specifically includes: there shall be no visible scars, cracks, sand holes, inclusions, pores and pinhole defects on the surface of the tube blank; batching principle: steel pipes shall be inspected and accepted in batches, and each batch shall consist of steel pipes of the same brand, same furnace number, same specification and same heat treatment system.

3. The method for preparing a high-pressure alloy boiler tube by online normalizing instead of offline normalizing heat treatment process technology according to claim 1, characterized in that: In the above 2), the discharging rhythm is controlled to be 54 pieces / second.

4. The method for preparing a high-pressure alloy boiler tube by online normalizing instead of offline normalizing heat treatment process technology according to claim 1, characterized in that: The continuous rolling piercing process includes: the piercing mill roll distance is 136mm, the guide plate distance is 156mm, the head position is 95-105mm, the rotation speed is 330-630rpm, the front pressing rate is 5.1%, the speed increase ratio is 1.9, the ovality is 1.15, and the outlet speed is 0.6m / s.

5. The method for preparing a high-pressure alloy boiler tube by online normalizing instead of offline normalizing heat treatment process technology according to claim 1, characterized in that: The chemical composition of the high-pressure alloy boiler tube is C: 0.12%, Si: 0.45%, Mn: 0.70%, P: 0.015%, S 0.005%, Mo: 0.35%, Ti: 0.06%, Cr: 1.50%, and the balance is Fe and unavoidable impurities.

6. The method for preparing a high-pressure alloy boiler tube by online normalizing instead of offline normalizing heat treatment process technology according to claim 1, characterized in that: The chemical composition of the high-pressure alloy boiler tube is C: 0.13%, Si: 0.48%, Mn: 0.80%, P: 0.007%, S 0.003%, Mo: 0.38%, Ti: 0.07%, Cr: 1.64%, and the balance is Fe and unavoidable impurities.

7. The method for preparing a high-pressure alloy boiler tube by online normalizing instead of offline normalizing heat treatment process technology according to claim 1, characterized in that: The chemical composition of the high-pressure alloy boiler tube is C: 0.14%, Si: 0.50%, Mn: 0.90%, P: 0.015%, S 0.005%, Mo: 0.40%, Ti: 0.08%, Cr: 1.70%, and the balance is Fe and unavoidable impurities.