Production method for producing SGCC steel plate at low cost

By adopting low-carbon and low-silicon process technology and controlled rolling and cooling technology in the production of SGCC steel plates, combined with annealing treatment and zinc liquid component control, the problem of low-cost production and insufficient adhesion of zinc layer is solved, and high performance and low cost are achieved The production of SGCC steel plates is in line with the development direction of energy-saving green steel.

CN119020566APending Publication Date: 2024-11-26BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411086318.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to produce SGCC steel plates with excellent performance at low cost, and the problems of leakage plating defects and insufficient adhesion of zinc layer are prone to occur during hot-dip galvanizing.

Method used

Using low-carbon and low-silicon technology, the cold rolling and rolling pressure reduction rate is controlled through high opening and rolling and low-temperature curling temperature, and the partition dispersion laminar flow is cooled, and activated aluminum is added during the annealing process. To improve the adhesion of zinc layer, simplify the smelting process, reduce energy consumption, and control the zinc liquid composition to reduce the formation of zinc slag.

Benefits of technology

It realizes the production of high-performance SGCC steel plates at low cost, improves the adhesion and anti-powdering capacity of the zinc layer, reduces production costs and energy consumption, simplifies the process flow, and meets the needs of multiple functional uses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004985277480000051
    Figure BDA0004985277480000051
  • Figure BDA0004985277480000061
    Figure BDA0004985277480000061
Patent Text Reader

Abstract

The invention discloses a low-cost production method for producing an SGCC steel plate, which is based on C-Mn, adopts a low-carbon and low-silicon process technology, and adopts a controlled rolling and controlled cooling process principle of high initial rolling temperature and low curling temperature in hot rolling; and the rolling reduction rate of cold rolling is controlled to be 65%-87%, so that the forming performance of the hot-dip galvanized substrate is guaranteed. The produced SGCC steel plate is low in cost and excellent in performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgical steel rolling, and in particular relates to a method for producing SGCC steel plates at low cost. Background Art

[0002] With the adjustment of the steel industry structure, it is imperative to develop deep processing, high value-added products and improve product competitiveness. Among them, the development of galvanized sheet and other coated products is one of the directions. The steel plate is hot-dip galvanized because zinc can play an anodic protection role on the steel plate in a corrosive environment and form a film with good corrosion resistance on the surface. The service life of the steel after hot-dip galvanizing is greatly extended. The good corrosion resistance of galvanized sheet has made it widely used. It is mainly used in construction, light industry, automobile, agriculture, animal husbandry, fishery, commerce and other industries. Among them: the construction industry uses galvanized sheet as industrial and civil building roof panels, ventilation ducts, light structures, etc. to prevent atmospheric corrosion; the light industry uses it to manufacture home appliance shells, civil chimneys, anti-theft doors and kitchen utensils, etc. Summary of the invention

[0003] The purpose of the present invention is to provide a low-cost production method for SGCC steel plates, which is based on C-Mn, adopts low-carbon and low-silicon process technology, and adopts the controlled rolling and controlled cooling process principle of high starting rolling temperature and low temperature curling temperature for hot rolling; the cold rolling reduction rate is controlled at 65% to 87% to ensure the forming performance of the hot-dip galvanized substrate. The produced SGCC steel plates are not only low in cost but also excellent in performance.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] The present invention provides a method for producing SGCC steel plates at low cost, comprising:

[0006] (1) heating a slab with a thickness of 67 to 72 mm to a temperature of 1050 to 1100° C. and keeping the temperature for 30 to 50 minutes (preferably 40 minutes);

[0007] (2) Hot rolling control starting rolling temperature greater than 1020 ℃, the final rolling temperature is 860 ~ 890 ℃; heating temperature, starting rolling temperature is 1030 ~ 1060 ℃,

[0008] (3) After hot rolling, the steel is cooled in an inter-group dispersed laminar cooling mode to control the cooling rate and intensity; the coiling temperature is 550-600°C;

[0009] (4) The cold rolling reduction rate is controlled at 60% to 87%;

[0010] (5) After cold rolling, the steel plate is laser welded by a welding machine, electrolytically degreased and cleaned, and then enters a non-oxidizing heating furnace for annealing heat treatment;

[0011] (6) Annealing temperature 700-850°C; reasonably control the holding time and cooling rate;

[0012] (7) The annealed steel sheet enters the zinc pot;

[0013] (8) After the steel plate comes out of the zinc pot, it is cooled in the cooling tower and then enters the leveling and straightening machine;

[0014] (9) The steel plates coming out of the straightening machine are subjected to surface passivation treatment and then packaged into finished coils;

[0015] The chemical components of the SGCC steel plate in weight percentage are: C: 0.04-0.07%, Si: 0.015-0.050%, Mn: 0.12-0.20%, P≤0.020%, S≤0.015%, Alt≥0.015%, and the rest are Fe and unavoidable inclusions.

[0016] Furthermore, the chemical composition of the SGCC steel plate in weight percentage is: C: 0.050%, Si: 0.023%, Mn: 0.14%, P: 0.008%, S: 0.003%, Alt: 0.022%, Als: 0.021%, and the rest is Fe and unavoidable inclusions.

[0017] Furthermore, the chemical composition of the SGCC steel plate in weight percentage is: C: 0.056%, Si: 0.015%, Mn: 0.17%, P: 0.013%, S: 0.005%, Alt: 0.026%, Als: 0.023%, and the rest is Fe and unavoidable inclusions.

[0018] Furthermore, the chemical composition of the SGCC steel plate in weight percentage is: C: 0.062%, Si: 0.021%, Mn: 0.17%, P: 0.006%, S: 0.007%, Alt: 0.036%, Als: 0.034%, and the rest is Fe and unavoidable inclusions.

[0019] Further, the chemical composition of the SGCC steel plate in weight percentage is: C: 0.062%, Si: 0.027%, Mn: 0.15%, P: 0.009%, S: 0.002%, Alt: 0.031%, Als: 0.030%, and the rest is Fe and unavoidable inclusions.

[0020] Further, the chemical composition of the SGCC steel plate in weight percentage is: C: 0.062%, Si: 0.033%, Mn: 0.15%, P: 0.017%, S: 0.004%, Alt: 0.031%, Als: 0.028%, and the rest is Fe and unavoidable inclusions.

[0021] The main purpose of the annealing section on the hot-dip galvanizing line is to eliminate work hardening, recover recrystallization, ensure the temperature of the strip entering the zinc pot, and reduce the surface of the strip. Since there will inevitably be iron oxides on the surface of the cold-rolled sheet, it is necessary to anneal in an atmosphere containing hydrogen to reduce the oxides to iron, which can improve the surface activity of the steel sheet and improve the wettability of the substrate to the zinc liquid. If the surface contains a large area of ​​oxides, it will reduce the wettability to the zinc liquid, resulting in leakage defects or deteriorating the adhesion of the zinc layer. For high-strength steel, since alloy elements are added to the steel, the oxides of the alloy elements will be enriched on the surface during the annealing process, resulting in serious leakage defects on the surface.

[0022] In order to improve the adhesion of the zinc layer, about 0.2% active aluminum is usually added to the zinc liquid, so that the Fe2Al5 transition layer can be preferentially formed between the substrate and the zinc layer, which is conducive to preventing the rapid reaction of zinc and iron to form a brittle zinc-iron alloy phase, and improving the adhesion and anti-powdering ability of the coating. The addition of aluminum can also prevent the formation of bottom slag in the zinc pot and generate controllable scum. When the strip moves in the zinc pot, if the zinc slag adheres to the surface of the strip, it will form an obvious zinc slag defect. Therefore, how to reduce the formation of zinc slag by controlling the composition of zinc liquid is a key technology in hot-dip galvanizing production.

[0023] Compared with the prior art, the beneficial technical effects of the present invention are:

[0024] 1. In today's fiercely competitive market, low cost and high return have become the criteria and goals pursued by all businesses. Under the condition of meeting product requirements, this product provides the base material for SGCC steel plates with hot-rolled plates produced by short processes. Adhere to the low-cost production route and adopt low-carbon and low-silicon process production technology based on C-Mn steel. Optimize the process flow to improve the comprehensive performance of steel plates. Provide excellent and environmentally friendly substrates for color coating production.

[0025] 2. The present invention adopts low-cost clean steel smelting technology based on the characteristics of high quality, high yield, low consumption and safety, simplifies the process and reduces energy consumption. Single slag operation is adopted to strengthen rapid slag formation, control the basicity of slag and prevent slag tapping and other subsequent control measures to reduce the P content in molten steel, thereby shortening the production cycle and improving economic benefits. Desulfurization is mainly carried out during the refining process, and desulfurization is carried out by electrode heating and white slag making. It prevents S from making the steel plate brittle and affecting the ductility and deep drawing properties of the steel plate.

[0026] 3. The present invention realizes the stable production of 1.00mm thick SGCC steel plates at low cost and compact production process rhythm by controlling the rolling and cooling processes. On the premise of meeting user requirements, it realizes the purpose of steel with the same chemical composition and multiple functional uses, reduces costs, simplifies production processes, improves production efficiency, reduces energy consumption, etc., which is in line with the development direction of developing economical, clean and green steel. DETAILED DESCRIPTION

[0027] Combined with examples, a low-cost production method of SGCC steel plate is further described in detail:

[0028] The steel with chemical composition design in Table 1 is selected as the raw material. The chemical composition of the steel billet adopts low desulfurization, converter smelting, refining, calcium treatment and other smelting processes. The size of the steel billet is: 67~72mm (thickness) × 1200mm (width). The slab is heated in a heating furnace, soaked, and hot rolled to control the starting rolling temperature and the final rolling temperature. The cooling rate is controlled after the steel plate is rolled; the steel plate after hot rolling is cold rolled after acid rolling; after the cold rolling is completed, it is laser welded by a welding machine and then cleaned in the cleaning section. The cleaned steel plate enters the non-oxidizing heating furnace for annealing heat treatment at a temperature of 700~850℃; the insulation time and cooling rate are reasonably controlled. The annealed steel plate enters the zinc pot, and after coming out of the zinc pot, it is cooled in the cooling tower and enters the flattening and straightening machine.

[0029] The annealing process of multi-step curve system is adopted to reasonably control the holding time and cooling time. The thickness of the finished steel plate is 1.00mm. The mechanical properties test is shown in Table 2.

[0030] Table 1 Chemical composition of steel in various embodiments of the present invention, wt%

[0031] Serial number C Si Mn P S Alt Als 1 0.050 0.023 0.14 0.008 0.003 0.022 0.021 2 0.056 0.015 0.17 0.013 0.005 0.026 0.023 3 0.062 0.021 0.17 0.006 0.007 0.036 0.034 4 0.062 0.027 0.15 0.009 0.002 0.031 0.030 5 0.062 0.033 0.15 0.017 0.004 0.031 0.028

[0032] Controlled rolling and controlled cooling mainly refers to the strict control of rolling and controlled cooling process parameters according to specifications, including: (1) the starting rolling temperature of the austenite recrystallization zone is 1030-1060℃, (2) the total rolling reduction rate is ≥87%, and the final rolling temperature is 860-890℃. (3) The cooling is carried out in the form of intermittent group dispersed laminar cooling, the cooling speed and strength are controlled, and the coiling temperature is 550-600℃. (4) The cold rolling reduction rate is controlled at 60%-87%. (5) The cleaned cold-rolled steel sheet enters the non-oxidizing heating furnace for annealing heat treatment, and the annealing temperature is 700-850℃; the insulation time and cooling rate are reasonably controlled. (6) The annealed steel sheet enters the zinc pot, and after coming out of the zinc pot, it is cooled in the cooling tower and then enters the flattening and straightening machine. After straightening, the surface is passivated and packaged into finished coils.

[0033] Table 2 Process parameters of steels in various embodiments of the present invention

[0034]

[0035] The experimental results of the low-cost production method of the SGCC steel plate of the present invention are listed in Table 3, from which it can be seen that the yield strength of the steel plate is not less than 305MPa, the tensile strength is greater than 350MPa, and the elongation is greater than 36.0%. There is no crack at a bending angle of 180°, which meets the standards and customer requirements.

[0036] Table 3 Experimental results of steels of various embodiments of the present invention

[0037]

[0038] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A low-cost production method for SGCC steel plates, Features: include: (1) Heat the slab with a thickness of 67-72 mm to 1050-1100° C. and keep it warm for 30-50 minutes; (2) Hot rolling control starting rolling temperature greater than 1020 ℃, the final rolling temperature is 860 ~ 890 ℃; heating temperature, starting rolling temperature is 1030 ~ 1060 ℃, (3) After hot rolling, the steel is cooled in an inter-group dispersed laminar cooling mode to control the cooling rate and intensity; the coiling temperature is 550-600°C; (4) The cold rolling reduction rate is controlled at 60% to 87%; (5) After cold rolling, the steel plate is laser welded by a welding machine, electrolytically degreased and cleaned, and then enters a non-oxidizing heating furnace for annealing heat treatment; (6) Annealing temperature 700-850°C; reasonably control the holding time and cooling rate; (7) The annealed steel sheet enters the zinc pot; (8) After the steel plate comes out of the zinc pot, it is cooled in the cooling tower and then enters the leveling and straightening machine; (9) The steel plates coming out of the straightening machine are subjected to surface passivation treatment and then packaged into finished coils; The chemical components of the SGCC steel plate in weight percentage are: C: 0.04-0.07%, Si: 0.015-0.050%, Mn: 0.12-0.20%, P≤0.020%, S≤0.015%, Alt≥0.015%, and the rest are Fe and unavoidable inclusions.

2. The method for producing SGCC steel plate at low cost according to claim 1, Features: The chemical components of the SGCC steel plate in weight percentage are: C: 0.050%, Si: 0.023%, Mn: 0.14%, P: 0.008%, S: 0.003%, Alt: 0.022%, Als: 0.021%, and the rest are Fe and unavoidable inclusions.

3. The method for producing SGCC steel plate at low cost according to claim 1, Features: The chemical components of the SGCC steel plate in weight percentage are: C: 0.056%, Si: 0.015%, Mn: 0.17%, P: 0.013%, S: 0.005%, Alt: 0.026%, Als: 0.023%, and the rest are Fe and unavoidable inclusions.

4. The method for producing SGCC steel plate at low cost according to claim 1, Features: The chemical components of the SGCC steel plate in weight percentage are: C: 0.062%, Si: 0.021%, Mn: 0.17%, P: 0.006%, S: 0.007%, Alt: 0.036%, Als: 0.034%, and the rest are Fe and unavoidable inclusions.

5. The method for producing SGCC steel plate at low cost according to claim 1, Features: The chemical components of the SGCC steel plate in weight percentage are: C: 0.062%, Si: 0.027%, Mn: 0.15%, P: 0.009%, S: 0.002%, Alt: 0.031%, Als: 0.030%, and the rest are Fe and unavoidable inclusions.

6. The method for producing SGCC steel plate at low cost according to claim 1, Features: The chemical components of the SGCC steel plate in weight percentage are: C: 0.062%, Si: 0.033%, Mn: 0.15%, P: 0.017%, S: 0.004%, Alt: 0.031%, Als: 0.028%, and the rest are Fe and unavoidable inclusions.