Treatment and reutilization process for solid waste of metal electrolytic refining
Through low-cost process steps, including oxygen heating, HCl treatment and ultraviolet irradiation, the problems of high energy consumption and precious metal loss in existing copper anode mud treatment are solved, and efficient recycling and high purity treatment of gold and silver are achieved, reducing the Environmental pollution.
Patent Information
- Application Number
- CN202411133996.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
Smart Images

Figure CN119020602A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal recovery, in particular to a process for treating and reusing solid waste from metal electrolytic refining. Background Art
[0002] Anode mud is the precipitate formed by other metals or elements due to various reasons when the anode is polarized during the metal electrolytic refining process. These metals or elements exist in the anode in the form of simple substances, alloys or compounds. Because their equilibrium potential is higher than the anode potential, they cannot ionize and enter the electrolyte, or although they can ionize and enter the electrolyte, they immediately form insoluble salts with the electrolyte and precipitate. In addition, some metals or elements will be partially oxidized to form insoluble compounds or simple substances.
[0003] The metal in the anode mud usually exists in the form of dispersed fine powder, which may adhere to the anode surface, precipitate at the bottom of the electrolytic cell, or be suspended in the electrolyte. In order to ensure the normal progress of the electrolysis process, the anode mud needs to be cleaned regularly. The cleaned anode mud is enriched with most of the precious metals and certain scattered elements in the ore, concentrate or flux, and has a very high comprehensive recovery value. For example, the anode mud produced in the process of copper and lead electrolytic refining is rich in gold and silver and has a very high value.
[0004] At present, the domestic copper anode mud treatment processes mainly include pyrometallurgical process and hydrometallurgical process. The pyrometallurgical process mainly includes three steps of roasting, smelting and refining, all of which need to be operated at high temperature, with high energy consumption and certain impact on the environment. The hydrometallurgical process mainly involves acid leaching, solvent extraction and precipitation separation. Although it has the advantages of short process, low energy consumption and environmental protection, the current smelting link is relatively backward and there are many uncertain factors. There is a possibility of precious metal loss, and the anode mud is prone to incomplete leaching during pickling before entering the medium frequency furnace for ingot casting. Summary of the invention
[0005] In order to solve the above technical defects, the present invention has developed a process for treating and reusing solid waste from metal electrolytic refining, which can efficiently purify and recover gold and silver in anode mud at low cost, and the recovered gold and silver are of high purity.
[0006] A process for treating and recycling solid waste from metal electrolytic refining, comprising the following steps:
[0007] S1: Pretreatment of electrolytic anode mud
[0008] The electrolytic anode mud is placed in an oxygen atmosphere and heated to obtain pre-oxidized electrolytic anode mud, the pre-oxidized electrolytic anode mud is immersed in an HCl solution, stirred and then allowed to stand, and then filtered and finely filtered to obtain a filtrate containing impurities and a filter residue containing gold and silver, the pH of the impurity filtrate is adjusted to be neutral, and then the metal chloride therein is reduced and recovered, and the filter residue containing gold and silver is washed to obtain the pre-impregnated electrolytic anode mud;
[0009] S2: Pre-leaching electrolytic anode mud to prepare gold powder and silver chloride precipitation
[0010] The pre-impregnated electrolytic anode mud is mixed with concentrated nitric acid and placed in a container, stirred while irradiating with ultraviolet rays, then filtered to obtain gold powder and silver-containing filtrate, dried the gold powder and then melted and cast ingots, the silver-containing filtrate is placed in a container, sodium chloride is added, stirred until no precipitate is generated, filtered and washed to obtain silver chloride precipitate;
[0011] S3: Leaching and reduction of silver ions
[0012] The silver chloride precipitate is mixed with the sodium sulfite solution and placed in a container. After adjusting the pH, the mixture is stirred at room temperature to obtain a silver immersion solution. Anionic polyacrylamide is added to the silver immersion solution. After stirring evenly, hydrazine hydrate and ascorbic acid are added. The pH is continuously adjusted and stirred until no more precipitate is generated in the solution. The solid silver powder is obtained by filtering and washing.
[0013] Furthermore, the pretreatment of electrolytic anode mud in step S1 comprises the following steps:
[0014] S1.1: placing the electrolytic anode mud in an atmosphere sintering furnace, introducing oxygen so that the oxygen content in the atmosphere sintering furnace is 25-30%, and then adjusting the temperature to 300-500° C. and heating for 1.5-2 hours to obtain pre-oxidized electrolytic anode mud;
[0015] S1.2: Place the pre-oxidation electrolytic anode mud in a container, add 3-5 times the mass of HCl solution to immerse the pre-oxidation electrolytic anode mud, stir for 25-30 minutes and then stand for 1-1.5 hours, filter and then fine filter the obtained filtrate to obtain a filtrate containing impurities and a filter residue containing gold and silver, add sodium hydroxide to the impurity filtrate to adjust the pH to neutral, then reduce and recover the metal chloride therein, wash the filter residue containing gold and silver with clean water until the pH of the clean water after washing is neutral, and obtain pre-impregnation electrolytic anode mud.
[0016] Further, step S2 pre-leaching electrolytic anode mud to prepare gold powder and silver chloride precipitation includes the following steps:
[0017] S2.1: Mix 3-4 parts by weight of pre-soaked electrolytic anode mud with 100-120 parts by weight of concentrated nitric acid and place them in a container. Place the container under an ultraviolet lamp and adjust the wavelength of the ultraviolet light to 365-400nm and the light intensity to 500-550mW / cm2 , continuously irradiating the container with ultraviolet light, then stirring at a speed of 300-350 rpm for 2-2.5 hours, and then filtering to obtain gold powder and silver-containing filtrate;
[0018] S2.2: After drying the gold powder, melt and cast it into ingots to recover the gold powder. Put the silver-containing filtrate in a container, add 2-3 parts by weight of sodium chloride, stir until no precipitate is generated, and obtain silver chloride precipitate after filtering and washing.
[0019] Furthermore, step S3 of leaching and reducing silver ions comprises the following steps:
[0020] S3.1: 1-2 parts by weight of silver chloride precipitate and 10-12 parts by weight of sodium sulfite solution are mixed in a container, the pH is adjusted to 9-10, and then stirred at a temperature of 25-30° C. and a stirring speed of 150-200 rpm for 1.5-2 hours to obtain a silver immersion solution;
[0021] S3.2: Add 4-6wt% of anionic polyacrylamide to the silver immersion solution, stir evenly, then add 30-40wt% of hydrazine hydrate and 10-20wt% of ascorbic acid, add sodium hydroxide to adjust the pH to 12-13, continue stirring the reaction until no more precipitate is generated in the solution, filter and wash to obtain solid silver powder.
[0022] Furthermore, the mass fractions of the components of the electrolytic anode mud in step S1.1 are: 84% silver, 12% gold, 2% copper, 0.4% lead, 0.6% antimony, 0.5% nickel, and 0.5% bismuth.
[0023] Furthermore, the concentration of the HCl solution in step S1.2 is 20-25%.
[0024] Furthermore, the concentration of concentrated nitric acid in step S2.1 is 10-12 mol / L.
[0025] Furthermore, the concentration of the sodium sulfite solution in step S3.1 is 200-250 g / L.
[0026] Furthermore, in step S3, the pH is adjusted by adding sodium hydroxide.
[0027] Furthermore, the anionic monomer of the anionic polyacrylamide in step S3.2 is acrylic acid, with an ionicity of 15-30 wt% and a molecular weight of 1×10 6 -1.8×10 7 .
[0028] The beneficial effects are as follows: 1. The present invention mixes the silver chloride precipitate with the sodium sulfite solution, and adjusts the pH so that the anions in the sodium sulfite solution are converted to SO3 2-exists in the form of Ag + Form a stable complex, and then promote the continuous conversion of AgCl into Ag + and Cl - Then, by adding anionic polyacrylamide with excellent dispersibility to the obtained silver immersion solution, it can not only selectively adhere to each crystal face of the silver powder, thereby stably dispersing the silver powder and preventing it from agglomerating, but also the negatively charged acrylic anion monomer ions are grafted on the carbon chain of polyacrylamide and can also bind to Ag. + Electrostatic attraction increases the local concentration of silver ions, promotes the reduction reaction, and improves Ag + The reduction efficiency can be improved to achieve efficient and low-cost recovery of silver in solid waste from metal electrolytic refining.
[0029] 2. The present invention mixes the pre-soaked electrolytic anode mud with concentrated nitric acid and uses a wavelength of 365-400nm and a light intensity of 500-550mW / cm 2 The nitric acid molecules are transformed into an excited state under the irradiation of ultraviolet rays, producing a more active intermediate nitrate free radical with stronger oxidizing ability, which can oxidize silver faster and more effectively, avoid incomplete pickling and leaching, and thus improve the recovery rate of solid silver powder and the purity of gold powder.
[0030] 3. The present invention first performs aerobic high-temperature calcination on the electrolytic anode mud, which can not only remove insoluble impurities, but also generate metal oxides from copper, lead, antimony, nickel and bismuth in the electrolytic anode mud. The metal oxides are not only easier to react with hydrochloric acid, but also the surface of the oxidized metal is rough and has a large specific surface area, which increases the contact area with hydrochloric acid, further accelerates the reaction rate and acid leaching effect, can greatly remove metal impurities in the subsequent pre-leaching electrolytic anode mud, improve the purity of the subsequently obtained gold powder and solid silver powder, prevent the subsequent influence on the nitric acid leaching effect, and improve the recovery rate of the solid silver powder. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a process flow chart for treating and reusing solid waste from metal electrolytic refining adopted in an embodiment of the present invention. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] A process for treating and recycling solid waste from metal electrolytic refining, such as Figure 1 As shown, the following steps are included:
[0035] S1: Pretreatment of electrolytic anode mud
[0036] S1.1: placing the electrolytic anode mud in an atmosphere sintering furnace, introducing oxygen so that the oxygen content in the atmosphere sintering furnace is 25%, and then adjusting the temperature to 300° C. and heating for 1.5 hours to obtain pre-oxidized electrolytic anode mud;
[0037] S1.2: The pre-oxidation electrolytic anode mud is placed in a container, and a 20% concentration HCl solution of 3 times the mass is added to immerse the pre-oxidation electrolytic anode mud. After stirring for 25 minutes, it is allowed to stand for 1 hour. After filtering, the obtained filtrate is finely filtered to obtain a filtrate containing impurities and a filter residue containing gold and silver. Sodium hydroxide is added to the impurity filtrate to adjust the pH to neutral, and then the metal chloride therein is reduced and recovered. The filter residue containing gold and silver is washed with clean water until the pH of the washed clean water is neutral to obtain the pre-impregnation electrolytic anode mud.
[0038] S2: Pre-leaching electrolytic anode mud to prepare gold powder and silver chloride precipitation
[0039] S2.1: Mix 3 parts by weight of pre-soaked electrolytic anode mud with 100 parts by weight of concentrated nitric acid with a concentration of 10 mol / L in a container, and place the container under an ultraviolet lamp. Adjust the wavelength of the ultraviolet light to 365 nm and the light intensity to 500 mW / cm 2 , continuously irradiating the container with ultraviolet light, then stirring at a speed of 300 rpm for 1.5 hours, and then filtering to obtain gold powder and silver-containing filtrate;
[0040] S2.2: After drying the gold powder, melt and cast it into ingots to recover the gold powder. Put the silver-containing filtrate in a container, add 2 parts by weight of sodium chloride, stir until no precipitate is generated, and obtain the silver chloride precipitate after filtering and washing.
[0041] S3: Leaching and reduction of silver ions
[0042] S3.1: 1 part by weight of silver chloride precipitate and 10 parts by weight of sodium sulfite solution with a concentration of 200 g / L are mixed in a container, the pH is adjusted to 9, and then stirred at a temperature of 25° C. and a stirring speed of 150 rpm for 2 hours to obtain a silver immersion solution;
[0043] S3.2: Add 4wt% of anionic polyacrylamide to the silver immersion solution, stir evenly, then add 30wt% of hydrazine hydrate and 10wt% of ascorbic acid, add sodium hydroxide to adjust the pH to 12, continue stirring the reaction until no more precipitate is generated in the solution, filter and wash to obtain solid silver powder.
[0044] Example 2
[0045] A process for treating and recycling solid waste from metal electrolytic refining, such as Figure 1 As shown, the following steps are included:
[0046] S1: Pretreatment of electrolytic anode mud
[0047] S1.1: placing the electrolytic anode mud in an atmosphere sintering furnace, introducing oxygen so that the oxygen content in the atmosphere sintering furnace is 25%, and then adjusting the temperature to 300° C. and heating for 1.5 hours to obtain pre-oxidized electrolytic anode mud;
[0048] S1.2: The pre-oxidation electrolytic anode mud is placed in a container, and 5 times the mass of 20% HCl solution is added to immerse the pre-oxidation electrolytic anode mud. After stirring for 25 minutes, it is allowed to stand for 1 hour. After filtering, the obtained filtrate is finely filtered to obtain a filtrate containing impurities and a filter residue containing gold and silver. Sodium hydroxide is added to the impurity filtrate to adjust the pH to neutral, and then the metal chloride therein is reduced and recovered. The filter residue containing gold and silver is washed with clean water until the pH of the washed clean water is neutral to obtain the pre-impregnation electrolytic anode mud.
[0049] S2: Pre-leaching electrolytic anode mud to prepare gold powder and silver chloride precipitation
[0050] S2.1: 4 parts by weight of pre-soaked electrolytic anode mud and 120 parts by weight of concentrated nitric acid with a concentration of 10 mol / L are mixed in a container, and the container is placed under an ultraviolet lamp, and the wavelength of the ultraviolet light is adjusted to 365 nm and the light intensity is 500 mW / cm 2 , continuously irradiating the container with ultraviolet light, then stirring at a speed of 300 rpm for 1.5 hours, and then filtering to obtain gold powder and silver-containing filtrate;
[0051] S2.2: After drying the gold powder, melt and cast it into ingots to recover the gold powder. Put the silver-containing filtrate in a container, add 3 parts by weight of sodium chloride, stir until no precipitate is generated, and obtain the silver chloride precipitate after filtering and washing.
[0052] S3: Leaching and reduction of silver ions
[0053] S3.1: 2 parts by weight of silver chloride precipitate and 12 parts by weight of sodium sulfite solution with a concentration of 200 g / L are mixed in a container, the pH is adjusted to 9, and then stirred at a temperature of 25° C. and a stirring speed of 150 rpm for 2 hours to obtain a silver immersion solution;
[0054] S3.2: Add 6 wt% of anionic polyacrylamide to the silver immersion solution, stir evenly, then add 40 wt% of hydrazine hydrate and 20 wt% of ascorbic acid, add sodium hydroxide to adjust the pH to 12, continue stirring the reaction until no more precipitate is generated in the solution, filter and wash to obtain solid silver powder.
[0055] Example 3
[0056] A process for treating and recycling solid waste from metal electrolytic refining, such as Figure 1 As shown, the following steps are included:
[0057] S1: Pretreatment of electrolytic anode mud
[0058] S1.1: placing the electrolytic anode mud in an atmosphere sintering furnace, introducing oxygen so that the oxygen content in the atmosphere sintering furnace is 30%, and then adjusting the temperature to 500° C. and heating for 2 hours to obtain pre-oxidized electrolytic anode mud;
[0059] S1.2: The pre-oxidation electrolytic anode mud is placed in a container, and 3 times the mass of 25% HCl solution is added to immerse the pre-oxidation electrolytic anode mud. After stirring for 30 minutes, it is allowed to stand for 1.5 hours. After filtering, the obtained filtrate is finely filtered to obtain a filtrate containing impurities and a filter residue containing gold and silver. Sodium hydroxide is added to the impurity filtrate to adjust the pH to neutral, and then the metal chloride therein is reduced and recovered. The filter residue containing gold and silver is washed with clean water until the pH of the washed clean water is neutral to obtain pre-impregnation electrolytic anode mud.
[0060] S2: Pre-leaching electrolytic anode mud to prepare gold powder and silver chloride precipitation
[0061] S2.1: Mix 3 parts by weight of pre-soaked electrolytic anode mud with 100 parts by weight of concentrated nitric acid with a concentration of 12 mol / L in a container, and place the container under an ultraviolet lamp. Adjust the wavelength of the ultraviolet light to 400 nm and the light intensity to 550 mW / cm 2 , continuously irradiating the container with ultraviolet light, then stirring at a speed of 350 rpm for 2 hours, and then filtering to obtain gold powder and silver-containing filtrate;
[0062] S2.2: After drying the gold powder, melt and cast it into ingots to recover the gold powder. Put the silver-containing filtrate in a container, add 2 parts by weight of sodium chloride, stir until no precipitate is generated, and obtain the silver chloride precipitate after filtering and washing.
[0063] S3: Leaching and reduction of silver ions
[0064] S3.1: 1 part by weight of silver chloride precipitate and 10 parts by weight of sodium sulfite solution with a concentration of 250 g / L are mixed in a container, the pH is adjusted to 10, and then stirred at a temperature of 30° C. and a stirring speed of 200 rpm for 2.5 hours to obtain a silver immersion solution;
[0065] S3.2: Add 4 wt% of anionic polyacrylamide to the silver immersion solution, stir evenly, then add 30 wt% of hydrazine hydrate and 10 wt% of ascorbic acid, add sodium hydroxide to adjust the pH to 13, continue stirring the reaction until no more precipitate is generated in the solution, filter and wash to obtain solid silver powder.
[0066] Comparative Example 1
[0067] Compared with Example 1, the difference of Comparative Example 1 is that anionic polyacrylamide is not added to the silver immersion solution in step S3.2 in Comparative Example 1, and the remaining steps are the same as those in Example 1.
[0068] Comparative Example 2
[0069] Compared with Example 1, the difference of Comparative Example 2 is that ultraviolet irradiation is not performed in step S2.1 of Comparative Example 2, and the remaining steps are the same as those of Example 1.
[0070] Comparative Example 3
[0071] Compared with Example 1, the difference of Comparative Example 3 is that in step S1.1 of Comparative Example 3, the electrolytic anode mud is not placed in an oxygen atmosphere for heating, and the remaining steps are the same as those of Example 1.
[0072] Experiment 1: 10 g of sample was taken, and gold powder and solid silver powder were prepared by the processes of Examples 1-3 and Comparative Examples 1-3, respectively. After weighing, the mass fractions of the components of the electrolytic anode mud were: 84% silver, 12% gold, 2% copper, 0.4% lead, 0.6% antimony, 0.5% nickel, and 0.5% bismuth. The recovery rates of gold and silver were calculated, and the purity of the prepared gold powder and solid silver powder was measured by a gold and silver detector. The data of the recovery rate and purity were recorded and tabulated, as shown in Table 1. It can be seen that the recovery rates of gold and silver in the embodiment are greater than those in Comparative Examples 1-3, indicating that adding anionic polyacrylamide to the silver impregnation solution, ultraviolet irradiation and heating the electrolytic anode mud in an oxygen atmosphere can improve the recovery rate of silver. At the same time, it can be seen that the purity of gold and silver in the embodiment is higher than that of Comparative Examples 2 and 3, which can prove that ultraviolet irradiation and heating the electrolytic anode mud in an oxygen atmosphere can also improve the purity of gold and silver.
[0073] Table 1: Gold and silver recovery and purity
[0074]
[0075] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A process for treating and recycling solid waste from metal electrolytic refining, characterized in that: The following steps are involved: S1: Pretreatment of electrolytic anode mud The electrolytic anode mud is placed in an oxygen atmosphere and heated to obtain pre-oxidized electrolytic anode mud, the pre-oxidized electrolytic anode mud is immersed in an HCl solution, stirred and then allowed to stand, and then filtered and finely filtered to obtain a filtrate containing impurities and a filter residue containing gold and silver, the pH of the impurity filtrate is adjusted to be neutral, and then the metal chloride therein is reduced and recovered, and the filter residue containing gold and silver is washed to obtain the pre-impregnated electrolytic anode mud; S2: Pre-leaching electrolytic anode mud to prepare gold powder and silver chloride precipitation The pre-impregnated electrolytic anode mud is mixed with concentrated nitric acid and placed in a container, stirred while irradiating with ultraviolet rays, then filtered to obtain gold powder and silver-containing filtrate, dried the gold powder and then melted and cast ingots, the silver-containing filtrate is placed in a container, sodium chloride is added, stirred until no precipitate is generated, filtered and washed to obtain silver chloride precipitate; S3: Leaching and reduction of silver ions The silver chloride precipitate is mixed with the sodium sulfite solution and placed in a container. After adjusting the pH, the mixture is stirred at room temperature to obtain a silver immersion solution. Anionic polyacrylamide is added to the silver immersion solution. After stirring evenly, hydrazine hydrate and ascorbic acid are added. The pH is continuously adjusted and stirred until no more precipitate is generated in the solution. The solid silver powder is obtained by filtering and washing.
2. The process for treating and reusing solid waste from metal electrolytic refining according to claim 1, characterized in that: Step S1: pretreatment of electrolytic anode mud, including the following steps: S1.1: placing the electrolytic anode mud in an atmosphere sintering furnace, introducing oxygen so that the oxygen content in the atmosphere sintering furnace is 25-30%, and then adjusting the temperature to 300-500° C. and heating for 1.5-2 hours to obtain pre-oxidized electrolytic anode mud; S1.2: Place the pre-oxidation electrolytic anode mud in a container, add 3-5 times the mass of HCl solution to immerse the pre-oxidation electrolytic anode mud, stir for 25-30 minutes and then stand for 1-1.5 hours, filter and then fine filter the obtained filtrate to obtain a filtrate containing impurities and a filter residue containing gold and silver, add sodium hydroxide to the impurity filtrate to adjust the pH to neutral, then reduce and recover the metal chloride therein, wash the filter residue containing gold and silver with clean water until the pH of the clean water after washing is neutral, and obtain pre-impregnation electrolytic anode mud.
3. The process for treating and reusing solid waste from metal electrolytic refining according to claim 1, characterized in that: Step S2 pre-leaching electrolytic anode mud to prepare gold powder and silver chloride precipitation includes the following steps: S2.1: Mix 3-4 parts by weight of pre-soaked electrolytic anode mud with 100-120 parts by weight of concentrated nitric acid and place them in a container. Place the container under an ultraviolet lamp and adjust the wavelength of the ultraviolet light to 365-400nm and the light intensity to 500-550mW / cm 2 , continuously irradiating the container with ultraviolet light, then stirring at a speed of 300-350 rpm for 1.5-2 hours, and then filtering to obtain gold powder and silver-containing filtrate; S2.2: After drying the gold powder, melt and cast it into ingots to recover the gold powder. Put the silver-containing filtrate in a container, add 2-3 parts by weight of sodium chloride, stir until no precipitate is generated, and obtain silver chloride precipitate after filtering and washing.
4. The process for treating and reusing solid waste from metal electrolytic refining according to claim 1, characterized in that: Step S3: leaching and reducing silver ions, comprising the following steps: S3.1: 1-2 parts by weight of silver chloride precipitate and 10-12 parts by weight of sodium sulfite solution are mixed in a container, the pH is adjusted to 9-10, and then stirred at a temperature of 25-30° C. and a stirring speed of 150-200 rpm for 2-2.5 hours to obtain a silver immersion solution; S3.2: Add 4-6wt% of anionic polyacrylamide to the silver immersion solution, stir evenly, then add 30-40wt% of hydrazine hydrate and 10-20wt% of ascorbic acid, add sodium hydroxide to adjust the pH to 12-13, continue stirring the reaction until no more precipitate is generated in the solution, filter and wash to obtain solid silver powder.
5. The process for treating and reusing solid waste from metal electrolytic refining according to claim 2, characterized in that: The mass fractions of the components of the electrolytic anode mud in step S1.1 are: 84% silver, 12% gold, 2% copper, 0.4% lead, 0.6% antimony, 0.5% nickel, and 0.5% bismuth.
6. The process for treating and reusing solid waste from metal electrolytic refining according to claim 2, characterized in that: The concentration of the HCl solution in step S1.2 is 20-25%.
7. The process for treating and reusing solid waste from metal electrolytic refining according to claim 3, characterized in that: The concentration of concentrated nitric acid in step S2.1 is 10-12 mol / L.
8. The process for treating and reusing solid waste from metal electrolytic refining according to claim 4, characterized in that: The concentration of the sodium sulfite solution in step S3.1 is 200-250 g / L.
9. The process for treating and reusing solid waste from metal electrolytic refining according to claim 4, characterized in that: The method of adjusting pH in step S3 is to add sodium hydroxide.
10. The process for treating and reusing solid waste from metal electrolytic refining according to claim 4, characterized in that: The anionic monomer of the anionic polyacrylamide in step S3.2 is acrylic acid, with an ionicity of 15-30wt% and a molecular weight of 1×10 6 -1.8×10 7 .