Method for efficiently recovering gold from thiosulfuric acid gold salt
Through the modification of graphene oxide and polyethyleneimine, graphene oxide dispersion liquid with high specific surface area and excellent dispersion is generated, which solves the problem of difficulty in adsorption of gold thiosulfate ion and achieves high efficiency and low cost gold Recycled, with high adsorption capacity and selectivity, suitable for large-scale applications.
Patent Information
- Application Number
- CN202411135645.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
Existing adsorption materials have difficulty in adsorbing gold thiosulfate ions, low adsorption capacity and poor selectivity, resulting in low recovery efficiency and high cost of gold thiosulfate.
The modified treatment of graphene oxide and polyethyleneimine is adopted to form an amine-modified graphene oxide dispersion through mixed reaction, and the adsorption and reduction of gold thiosulfate ions are used to utilize its high specific surface area and excellent dispersion. Directly obtain the gold element.
It realizes efficient and low-cost gold thiosulfate ion recovery, with high adsorption capacity and excellent selectivity, no additional reducing agent required, and is simple in process and suitable for large-scale applications.
Smart Images

Figure CN119020603A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of precious metal resource recovery, and in particular relates to a method for efficiently recovering gold from gold thiosulfate salt. Background Art
[0002] Gold is widely used in electronic products and consumer products as a good conductor of electricity. Its natural scarcity determines the importance of sustainable development of gold resources. Recycling and reusing waste gold resources is an effective means to achieve sustainable development of gold resources. Compared with the traditional cyanide method for gold extraction, the thiosulfate leaching method has gradually attracted attention due to its advantages of green environmental protection and high leaching efficiency. The adsorption method is simple to operate, low in energy consumption and high in efficiency, and is currently the most commonly used method in the field of resource recovery. However, the high charge density and large size of gold thiosulfate make it difficult to recover. Most adsorption materials are difficult to achieve effective adsorption and recovery of gold thiosulfate ions. For example, the adsorption capacity of modified activated carbon materials for gold thiosulfate ions is less than 10 mg / g, and gold thiosulfate ions cannot be directly reduced to gold. Additional reducing agents need to be added, and the selectivity is poor, which further increases the complexity and cost of the recovery process. Therefore, it is still challenging to develop materials with high adsorption capacity and selectivity to achieve efficient extraction and recovery of gold thiosulfate.
[0003] It should be noted that the information disclosed in the above background technology section is only used for understanding the background of the present application, and therefore may include information that does not constitute prior art known to ordinary technicians in the field. Summary of the invention
[0004] In order to solve the technical problems that existing adsorption materials are difficult to adsorb gold thiosulfate ions, have low adsorption capacity and poor selectivity, the present invention provides a method for efficiently recovering gold from gold thiosulfate salts.
[0005] The technical solution of the present invention to solve the above technical problems is as follows:
[0006] A method for efficiently recovering gold from gold thiosulfate salt comprises the following steps: S1, mixing a graphene oxide dispersion liquid and a polyethyleneimine aqueous solution for reaction; S2, washing the reaction liquid of step S1 multiple times to obtain a polyethyleneimine-modified graphene oxide dispersion liquid; S3, mixing a solution containing gold thiosulfate ions and the dispersion liquid to obtain an initial reaction liquid, and reacting under stirring so that the polyethyleneimine-modified graphene oxide in the dispersion liquid adsorbs and reduces the gold thiosulfate ions to obtain gold; S4, washing and drying the reaction liquid obtained in step S3, and then calcining at high temperature in an oxygen-containing atmosphere to obtain pure gold.
[0007] Preferably, in the step S1, the mass ratio of the polyethyleneimine to the graphene oxide is 1-1000:1.
[0008] Preferably, in step S1, the average molecular weight of the polyethyleneimine is 600-75000, and the molecular structure is branched or linear.
[0009] Preferably, in step S4, the calcination temperature is 300-1300° C., and the calcination time is 0.1-6 hours.
[0010] Preferably, in step S3, the concentration of gold ions in the solution containing gold ions is 0.001-10000 mg / L.
[0011] Preferably, the solution containing gold thiosulfate ions in step S3 is a solution containing gold thiosulfate ions alone.
[0012] Preferably, the solution containing gold thiosulfate ions in step S3 is a mixed solution containing gold thiosulfate ions and other ions.
[0013] Preferably, the solution containing gold thiosulfate ions is gold electroplating waste liquid, gold ore or leaching liquid of electronic waste.
[0014] Preferably, in step S3, the pH of the initial reaction solution is 5-14.
[0015] The beneficial effects of the present invention include: in the method of the present invention, polyethyleneimine is used to modify graphene oxide to prepare an amine-modified graphene oxide dispersion by a chemical method, the graphene oxide mainly plays the role of high specific surface area and excellent dispersibility, provides sufficient adsorption sites, and the amine group plays its excellent reducing role, which is helpful to efficiently recover gold from the gold ion-containing solution. It is proved by experiments that the graphene oxide modified by polyethyleneimine realizes a reducing adsorption effect on gold thiosulfate ions, and can directly and efficiently reduce the gold thiosulfate ions to obtain gold element, and has a high adsorption capacity and excellent selectivity. The method of the present invention is simple in process, and the obtained adsorption material has excellent gold ion selectivity, and can directly reduce the gold thiosulfate ions to gold element without additional reducing agent, is green and environmentally friendly, and has low cost, can realize the adsorption and recovery of high-purity gold elements, and is conducive to large-scale application. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 3 is a graph showing the variation of the adsorption capacity of the dispersion in Example 1 of the present invention for gold thiosulfate ions with the concentration of gold ions.
[0017] Figure 2 This is a scanning electron microscope image of the dispersion in Example 1 of the present invention after adsorption and reduction of gold thiosulfate ions.
[0018] Figure 3 This is an X-ray diffraction diagram of the dispersion in Example 1 of the present invention after adsorption and reduction of gold thiosulfate ions.
[0019] Figure 4 It is a performance diagram of gold selective recovery of the dispersion in Examples 4 and 5 of the present invention in the presence of competing ions. DETAILED DESCRIPTION
[0020] The present invention can be better understood according to the following examples. However, it is easy for those skilled in the art to understand that the contents described in the examples are only used to illustrate the present invention, and should not and will not limit the present invention described in the claims. In the following, ppm represents mg / L.
[0021] The specific embodiment of the present invention provides a method for efficiently recovering gold from thiosulfate gold salt, which comprises the following steps: S1, mixing a graphene oxide dispersion and a polyethyleneimine aqueous solution for reaction; S2, washing the reaction solution of step S1 multiple times to obtain a dispersion of polyethyleneimine-modified graphene oxide; S3, mixing a solution containing gold thiosulfate ions and the dispersion to obtain an initial reaction solution, and reacting under stirring so that the polyethyleneimine-modified graphene oxide in the dispersion adsorbs and reduces the gold thiosulfate ions, and the polyethyleneimine-modified graphene oxide has a reductive adsorption effect on the gold thiosulfate ions, and can reduce the gold ions to obtain gold element; S4, washing and drying the reaction solution obtained in step S3, and then calcining at high temperature in an oxygen-containing atmosphere to obtain elemental pure gold.
[0022] In a preferred embodiment, in the step S1, the mass ratio of the polyethyleneimine to the graphene oxide is 1-1000: 1. In the step S1, the graphene oxide dispersion (water as solvent) is added dropwise to the polyethyleneimine aqueous solution, stirred while adding, and mixed evenly to obtain the polyethyleneimine-modified graphene oxide dispersion.
[0023] In a preferred embodiment, in the step S1, the average molecular weight of the polyethyleneimine is 600-75000, and the molecular structure is branched or linear.
[0024] In a preferred embodiment, in step S4, the calcination temperature is 300-1300° C., and the calcination time is 0.1-6 hours.
[0025] In a preferred embodiment, in step S3, the concentration of gold ions in the solution containing gold ions is 0.001-10000 mg / L.
[0026] In a preferred embodiment, the solution containing gold thiosulfate ions in step S3 is a solution containing gold thiosulfate ions alone.
[0027] In a preferred embodiment, the solution containing gold thiosulfate ions in step S3 is a mixed solution containing gold thiosulfate ions and other ions.
[0028] In a preferred embodiment, the solution containing gold thiosulfate ions is gold electroplating waste liquid, gold ore or leaching liquid of electronic waste.
[0029] In a preferred embodiment, in step S3, the pH of the initial reaction solution is 5 to 14. The present invention is described in more detail below through some specific examples.
[0030] Example 1
[0031] (1) adding graphene oxide dispersion dropwise into polyethyleneimine aqueous solution and stirring and mixing, wherein the mass ratio of polyethyleneimine to graphene oxide is 120:1, the average molecular weight of the polyethyleneimine is 25000, and the molecular structure is branched.
[0032] (2) After washing the reaction solution of graphene oxide and polyethyleneimine for multiple times, a dispersion solution containing polyethyleneimine-modified graphene oxide is obtained, and the concentration of the dispersion solution is 1 mg / mL.
[0033] (3) 0.4 mL of a dispersion of polyethyleneimine-modified graphene oxide was added to 200 mL of an aqueous solution containing single gold thiosulfate ions at a concentration of 10 ppm to obtain an initial reaction solution. The pH of the initial reaction solution was 8. After a certain period of stirring and reacting, the polyethyleneimine-modified graphene oxide achieved the highest adsorption of gold thiosulfate.
[0034] (4) The product is centrifuged, washed, and dried, and then calcined at 800°C in an air atmosphere for 2 hours to obtain pure gold.
[0035] The same method as in Example 1 was used to adsorb the aqueous solutions of gold thiosulfate ions at concentrations of 0.05 ppm, 1 ppm, 50 ppm and 100 ppm, respectively. The adsorption capacity of the dispersion obtained in step (2) for gold thiosulfate ions varied with the concentration of gold ions as shown in the following table: Figure 1 As shown, from Figure 1 It can be seen that the dispersion obtained in step (2) of this embodiment has an adsorption capacity of up to 879 mg / g when the gold thiosulfate concentration is a trace amount of 10 ppm, and still has a relatively high adsorption capacity at a concentration below 10 ppm; Figure 2 and Figure 3It can be seen that the polyethyleneimine-modified graphene oxide of the present invention has a reductive adsorption on gold thiosulfate ions, and can directly reduce the gold ions into gold elements.
[0036] Example 2
[0037] (1) adding graphene oxide dispersion dropwise into polyethyleneimine aqueous solution and stirring and mixing, wherein the mass ratio of polyethyleneimine to graphene oxide is 1:1, the average molecular weight of the polyethyleneimine is 600, and the molecular structure is linear.
[0038] (2) After washing the reaction solution of graphene oxide and polyethyleneimine for multiple times, a dispersion solution containing polyethyleneimine-modified graphene oxide is obtained, and the concentration of the dispersion solution is 1 mg / mL.
[0039] (3) 0.4 mL of a dispersion of polyethyleneimine-modified graphene oxide was added to 200 mL of an aqueous solution containing single gold thiosulfate ions at a concentration of 0.001 ppm to obtain an initial reaction solution. The pH of the initial reaction solution was 5. After a certain period of stirring and reacting, the polyethyleneimine-modified graphene oxide achieved the highest adsorption of gold thiosulfate.
[0040] (4) The product is centrifuged, washed, dried, and then calcined at 300°C in an oxygen atmosphere for 6 hours to obtain pure gold.
[0041] Example 3
[0042] (1) Adding graphene oxide dispersion dropwise into polyethyleneimine aqueous solution and stirring to mix, wherein the mass ratio of polyethyleneimine to graphene oxide is 1000:1, the average molecular weight of the polyethyleneimine used is 75000, and the molecular structure is branched.
[0043] (2) After washing the reaction solution of graphene oxide and polyethyleneimine for multiple times, a dispersion solution containing polyethyleneimine-modified graphene oxide is obtained, and the concentration of the dispersion solution is 1 mg / mL.
[0044] (3) 0.4 mL of a dispersion of polyethyleneimine-modified graphene oxide was added to 200 mL of an aqueous solution containing single gold thiosulfate ions at a concentration of 10,000 ppm. The pH of the solution was 14. After a certain period of stirring and reaction, the polyethyleneimine-modified graphene oxide achieved the highest adsorption of gold thiosulfate.
[0045] (4) The product is centrifuged, washed, and dried, and then calcined at 1300°C in an oxygen atmosphere for 0.1 hour to obtain pure gold.
[0046] Example 4
[0047] (1) to (2) are respectively the same as steps (1) to (2) of Example 1.
[0048] (3) Selectively recovering gold thiosulfate from gold electroplating waste liquid using the dispersion obtained in step (2): adding 0.4 mL of the dispersion to 200 mL of an aqueous solution containing 10 ppm of gold thiosulfate ions, 5200 ppm of sodium ions, 6450 ppm of thiosulfate ions and 4600 ppm of sulfite ions, mixing evenly, the solution pH = 8, and stirring for a certain period of time to react.
[0049] (4) The product is centrifuged, washed, and dried, and then calcined at 900°C in an air atmosphere for 2 hours to obtain pure gold.
[0050] Example 5
[0051] (1) to (2) are respectively the same as steps (1) to (2) of Example 1.
[0052] (3) Selectively recovering gold thiosulfate from gold electroplating waste liquid using the dispersion obtained in step (2): adding 0.4 mL of the dispersion to 200 mL of an aqueous solution containing 110 ppm of gold thiosulfate ions, 5200 ppm of sodium ions, 6450 ppm of thiosulfate ions and 4600 ppm of sulfite ions, mixing evenly, the solution pH = 8, and stirring for a certain period of time to react.
[0053] (4) The product is centrifuged, washed, and dried, and then calcined at 900°C in an air atmosphere for 2 hours to obtain pure gold.
[0054] The test results of the selective recovery of gold in the dispersions of Examples 4 and 5 in the presence of competing ions show that the dispersions can still highly selectively recover gold (the adsorption of sodium ions is less than 10 mg / g) in an environment containing other competing ions. The performance diagram is shown in FIG. Figure 4 As shown, it can be seen that the polyethyleneimine-modified graphene oxide of the present invention can still highly selectively recover gold thiosulfate in an environment containing other high-concentration competing ions, and has great application potential.
[0055] Example 6
[0056] (1) to (2) are respectively the same as steps (1) to (2) of Example 1.
[0057] (3) The dispersion obtained in step (2) is used to selectively recover gold thiosulfate from a gold ore leachate: 0.4 mL of the dispersion is added to 200 mL of an aqueous solution containing 10 ppm of gold thiosulfate ions, 2560 ppm of copper ions, 18400 ppm of sodium ions, 44800 ppm of thiosulfate ions and 16000 ppm of sulfite ions, and the mixture is mixed evenly. The solution has a pH of 8. After a certain period of stirring and reacting, the dispersion can still highly selectively recover gold in an environment containing other competing ions (the adsorption of sodium ions and copper ions is less than 10 mg / g).
[0058] (4) The product is centrifuged and dried, and then calcined at 800°C in an air atmosphere for 3 hours to obtain pure gold.
[0059] It can be seen from the above examples that the adsorbent material of the present invention has a high adsorption capacity and excellent selectivity for gold thiosulfate ions, and can directly reduce gold thiosulfate ions to gold element efficiently, and can efficiently recover gold from gold-containing solutions, gold electroplating waste liquid and gold ore leaching liquid. It has great application potential in solving the sustainable challenge of global gold recyclability.
[0060] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art of the present invention, several equivalent substitutions or obvious variations can be made without departing from the concept of the present invention, and the performance or use is the same, which should be regarded as belonging to the protection scope of the present invention.
Claims
1. A method for efficiently recovering gold from gold thiosulfate salts, It is characterized in that The steps include: S1, mixing a graphene oxide dispersion and a polyethyleneimine aqueous solution for reaction; S2, washing the reaction solution of step S1 multiple times to obtain a dispersion of polyethyleneimine-modified graphene oxide; S3, mixing a solution containing gold thiosulfate ions and the dispersion to obtain an initial reaction solution, and reacting under stirring so that the polyethyleneimine-modified graphene oxide in the dispersion adsorbs and reduces the gold thiosulfate ions to obtain gold element; S4. After washing and drying the reaction solution obtained in step S3, calcining at high temperature in an oxygen-containing atmosphere can obtain pure gold.
2. The method for efficiently recovering gold from thiosulfate gold salt as claimed in claim 1, It is characterized in that In the step S1, the mass ratio of the polyethyleneimine to the graphene oxide is 1-1000:
1.
3. The method for efficiently recovering gold from thiosulfate gold salt as claimed in claim 1, It is characterized in that In the step S1, the average molecular weight of the polyethyleneimine is 600-75000, and the molecular structure is branched or linear.
4. The method for efficiently recovering gold from thiosulfate gold salt as claimed in claim 1, It is characterized in that In the step S4, the calcination temperature is 300-1300° C., and the calcination time is 0.1-6 hours.
5. The method for efficiently recovering gold from thiosulfate gold salt as claimed in claim 1, It is characterized in that In step S3, the concentration of gold thiosulfate ions in the solution containing gold thiosulfate ions is 0.001-10000 mg / L.
6. The method for efficiently recovering gold from a solution containing gold thiosulfate ions as claimed in claim 1, It is characterized in that The solution containing gold thiosulfate ions in step S3 is a solution containing gold thiosulfate ions alone.
7. The method for efficiently recovering gold from a solution containing gold thiosulfate ions as claimed in claim 1, It is characterized in that The solution containing gold thiosulfate ions in step S3 is a mixed solution containing gold thiosulfate ions and other ions.
8. A method for efficiently recovering gold from a solution containing gold thiosulfate ions as claimed in claim 7, It is characterized in that The mixed solution containing gold thiosulfate ions and other ions is gold electroplating waste liquid, gold ore or leaching liquid of electronic waste.