Ultrahigh-strength Cu15Ni8Sn alloy for aviation knuckle bearing and preparation method of bar of ultrahigh-strength Cu15Ni8Sn alloy

By preparing large-scale ultra-high-strength Cu15Ni8Sn alloy rods, combined with electromagnetic casting and precision forging technology, the problem of difficult to produce copper alloys for large-scale aviation joint bearings in China has been solved, high strength and wear resistance are achieved, and beryllium copper is replaced. Materials meet high-performance needs in aerospace and other fields.

CN119020633APending Publication Date: 2024-11-26HUNAN HI-TECH CUWAY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411144020.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The industrial production of ultra-high strength Cu15Ni8Sn alloys for large-scale aviation joint bearings has not yet been achieved in China, and the shortage of supply of beryllium bronze and the rising price have forced the search for alternatives to high-strength, wear-resistant and corrosion-resistant environmentally friendly copper alloy materials.

Method used

14.5% to 16% Ni, 7.5% to 8.5% Sn, ≤0.2% Si, 0.3≤% Zn, ≤0.2% Mg, ≤0.3% Mn, ≤0.1% Nb were used, and the margin was Copper proportional smelting, combined with electromagnetic casting, rapid free forging, solid solution treatment, fine forging and aging annealing, large-scale ultra-high strength Cu15Ni8Sn alloy rods are prepared.

Benefits of technology

The production of ultra-high strength copper-nickel-tin alloy rods for aviation joint bearings has been realized, with tensile strength ≥1200MPa, yield strength ≥1105MPa, hardness ≥38HRC, elongation ≥3%, satisfying high load, wear resistance and impact resistance and the application requirements for thermal conductivity have replaced beryllium bronze material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020633A_ABST
    Figure CN119020633A_ABST
Patent Text Reader

Abstract

The ultrahigh-strength Cu15Ni8Sn alloy for the aviation knuckle bearing comprises the following components in percentage by mass: 14.5%-16% of Ni, 7.5%-8.5% of Sn, smaller than or equal to 0.2% of Si, smaller than or equal to 0.3% of Zn, smaller than or equal to 0.2% of Mg, smaller than or equal to 0.3% of Mn, smaller than or equal to 0.1% of Nb and the balance of Cu and inevitable impurities. The machining method comprises the unique combined machining process of vertical semi-continuous electromagnetic casting, sawing and slitting, homogenization and rapid free forging, solution treatment, precision forging, straightening and sawing, aging treatment and stress relief annealing. According to the ultrahigh-strength Cu15Ni8Sn alloy for the aviation knuckle bearing and the preparation method of the ultrahigh-strength Cu15Ni8Sn alloy bar, collaborative optimization of components and the process is completed, the maximum product of strength and elongation is achieved, and therefore the wear resistance of the Cu15Ni8Sn alloy is improved, replacement of beryllium bronze (C17200) alloy in the aviation knuckle bearing is completed, and the service life of the aviation knuckle bearing is prolonged. And the application requirements of high load, friction resistance, impact resistance and heat conduction of the aircraft landing gear at an extremely low temperature are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper alloy materials, and in particular to an ultra-high-strength Cu15Ni8Sn alloy for aviation spherical bearings and a method for preparing a rod thereof. Background Art

[0002] Spherical plain bearings are spherical sliding bearings whose sliding contact surfaces are an inner spherical surface and an outer spherical surface, which can rotate and swing at any angle. Spherical plain bearings have the characteristics of large load capacity, impact resistance, corrosion resistance, wear resistance, self-aligning, and good lubrication. The outer spherical surface is made of high-strength steel, and the inner spherical surface is made of high-strength and wear-resistant beryllium bronze alloy (C17200).

[0003] With the development of industries such as aerospace, petrochemical, and communications electronics, the use environment of materials is becoming more and more complex and the application requirements are becoming more and more stringent. As the key material for the inner spherical surface of spherical bearings, it requires high load, impact resistance, corrosion resistance, wear resistance, self-alignment, good lubrication, etc. At present, beryllium bronze is still a typical representative of high-strength, high-elasticity, and wear-resistant copper alloy materials, and is also widely used in aerospace and petrochemical fields. With the international call for and prohibition of the use of beryllium copper, and the increasingly tense international situation, beryllium bronze as a war reserve resource has been in the planned market product, resulting in a shortage of beryllium copper master alloy supply and a continuous increase in the price of beryllium copper products, forcing application customers to urgently find a high-strength, wear-resistant, and corrosion-resistant environmentally friendly copper alloy material to replace beryllium bronze, which is already a general trend.

[0004] Nickel-tin alloy (such as Cu-15Ni-8Sn) is a high-end copper alloy material with high strength, excellent wear resistance and corrosion resistance. In particular, the strength of Cu-15Ni-8Sn alloy can reach over 1300MPa, which is comparable to high-strength steel and beryllium bronze. Its corrosion resistance in seawater or acidic and oil and gas environments and its wear resistance under high load conditions are better than those of beryllium bronze and aluminum bronze. It is an ideal material to replace beryllium bronze.

[0005] At present, key technologies such as copper-nickel-tin alloy smelting and casting segregation, coarse processing structure, and heat treatment cracking are bottlenecks restricting domestic copper processing enterprises. The country can only achieve small-batch supply of products with a diameter of less than 120 mm, and no other company can achieve industrial production of large-size products. Therefore, developing a large-size (φ150mm) ultra-high strength Cu15Ni8Sn alloy product to replace imports and fill the domestic gap to promote the development of high-strength, wear-resistant and environmentally friendly copper alloy technology is a technical problem that urgently needs to be solved in this field. Summary of the invention

[0006] The invention discloses an ultra-high-strength Cu15Ni8Sn alloy for aviation spherical bearings and a rod preparation method thereof, aiming to solve the technical problems in the background technology.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] The invention discloses an ultra-high strength Cu15Ni8Sn alloy for aviation spherical bearings, comprising the following components in percentage by mass: 14.5% to 16% Ni, 7.5% to 8.5% Sn, ≤0.2% Si, 0.3% to ≤% Zn, ≤0.2% Mg, ≤0.3% Mn, ≤0.1% Nb, and the balance of Cu and unavoidable impurities.

[0009] A method for preparing an ultra-high strength Cu15Ni8Sn alloy bar for aviation spherical bearings, specifically comprising the following steps:

[0010] Step 1: Smelting: Smelt according to the ratio of 14.5% to 16% Ni, 7.5% to 8.5% Sn, ≤0.2% Si, 0.3≤% Zn, ≤0.2% Mg, ≤0.3% Mn, ≤0.1% Nb, and the balance is copper, add charcoal to cover and protect, then stand and heat to 1280℃~1300℃; Nb is added to the holding furnace in the form of CuNb master alloy, then calcine charcoal to cover, measure and adjust the temperature, and then take samples for testing;

[0011] Step 2: electromagnetic casting: adjust the temperature of the holding furnace to 1260℃~1280℃, the magnetic field to 30-40HZ, set the normal pulling casting speed to 80mm / min~90mm / min, and after the casting is completed, the copper alloy billet is obtained, and the grain size of the organization is 50~100μm;

[0012] Step 3: sawing and segmenting: saw off 50mm to 80mm from the head and tail of the copper alloy billet obtained in step 2, and then sawing it into 500mm to 600mm / segment;

[0013] Step 4: Homogenization + rapid free forging: The copper alloy billet obtained by sawing in step 3 is subjected to high temperature and long-term homogenization at 850℃~860℃ for 8~10h; rapid free forging is performed in a 1200T rapid forging machine to reduce the extreme temperature loss during the process, ensure that the final forging temperature is greater than 600℃, and obtain a copper alloy bar with a diameter and a microstructure grain size of 30~50μm;

[0014] Step 5: Solution treatment: The copper alloy rod obtained in step 4 is kept at 850°C to 860°C for 4 hours, and then quickly quenched to obtain a supersaturated solution copper alloy rod;

[0015] Step 6: Precision forging: The bar obtained in step 5 is subjected to high-frequency cold precision forging in a 260T precision forging machine, with the pass processing controlled at 10% to 15% and the total processing deformation less than 40%;

[0016] Step 7: Straightening and sawing: Straighten the bars obtained in step 6 and cut them into 90mm long bars;

[0017] Step 8: Aging treatment: The bar obtained in step 7 is subjected to aging treatment at 380-400°C for 2.5 hours to strengthen the performance of the copper alloy bar;

[0018] Step 9: Stress relief annealing: The rod obtained in step 8 is kept at 260-270°C for 4 hours for stress relief annealing to eliminate the internal stress of the material and obtain the copper alloy rod with maximum strength and plasticity.

[0019] The ultra-high strength Cu15Ni8Sn alloy and rod preparation method for aviation joint bearings provided by the present invention utilizes the combination of traditional free forging and advanced precision forging equipment processes, and cooperates with a suitable heat treatment strip decomposition process to effectively solve the problem of large-scale cold and hot processing. At the same time, the alloy after aging contains a large number of dispersed nano-reinforced particles, which promote the pinning dislocation to hinder its movement, thereby improving the hardness, strength and other performance indicators of the alloy, and finally obtains large-scale ultra-high strength copper-nickel-tin alloy rods, achieving the maximum strength-plastic product of strength and elongation, tensile strength ≥1200MPa, yield strength ≥1105MPa, hardness ≥38HRC, and elongation ≥3%. The replacement of beryllium bronze (C17200) alloy in aviation joint bearings is completed, meeting the application requirements of high load, wear resistance, impact resistance and heat conduction at extremely low temperatures in aircraft landing gear. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is an overall flow chart of a method for preparing an ultra-high-strength Cu15Ni8Sn alloy and a rod thereof for aviation spherical bearings proposed by the present invention. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0022] Reference Figure 1 , a method for preparing an ultra-high-strength Cu15Ni8Sn alloy and a rod thereof for aviation spherical bearings, comprising the following steps:

[0023] 1) Smelting: Smelt in the proportion of 14.5% to 16% Ni, 7.5% to 8.5% Sn, ≤0.2% Si, 0.3≤% Zn, ≤0.2% Mg, ≤0.3% Mn, ≤0.1% Nb, and the balance is copper, cover with charcoal for protection, and then stand and heat to 1280°C to 1300°C; Nb is added to the holding furnace in the form of CuNb master alloy, and then calcined with charcoal, covered, measured and adjusted, and then sampled for testing;

[0024] 2) Electromagnetic casting: adjust the holding furnace temperature to 1260℃~1280℃, the magnetic field to 30-40HZ, set the normal pulling casting speed to 80mm / min~90mm / min, and obtain the copper alloy billet after casting, with a grain size of 50~100μm;

[0025] 3) Sawing and segmenting: sawing off 50 mm to 80 mm from the head and tail of the copper alloy bar blank obtained in step 2), and then sawing into 500 mm to 600 mm / segment;

[0026] 4) Homogenization + rapid free forging: The copper alloy bar blank obtained by sawing in step 3) is subjected to high temperature and long-term homogenization at 850°C to 860°C for 8 to 10 hours; rapid free forging is performed in a 1200T rapid forging machine to reduce the extreme temperature loss during the process, ensure that the final forging temperature is greater than 600°C, and obtain a copper alloy bar with a diameter and a microstructure grain size of 30 to 50 μm;

[0027] 5) Solution treatment: the copper alloy rod obtained in step 4) is kept at 850° C. to 860° C. for 4 hours, and then rapidly quenched to obtain a supersaturated solution copper alloy rod;

[0028] 6) Precision forging: The bar obtained in step 5) is subjected to high-frequency cold precision forging in a 260T precision forging machine, with the pass processing controlled at 10% to 15%, and the total processing deformation less than 40%;

[0029] 7) Straightening and sawing: straighten the bars obtained in step 6) and cut them into bars with a length of 90 mm;

[0030] 8) Aging treatment: The bar obtained in step 7) is subjected to aging treatment at 380-400°C for 2.5 hours to strengthen the performance of the copper alloy bar;

[0031] 9) Stress relief annealing: The rod obtained in step 8) is kept at 260-270° C. for 4 hours for stress relief annealing to eliminate the internal stress of the material and obtain a copper alloy rod with maximum strength and plasticity.

[0032] Example 1

[0033] 1. A method for preparing an ultra-high-strength Cu15Ni8Sn alloy and a rod thereof for aviation spherical bearings, characterized in that it comprises the following steps:

[0034] 1) Smelting: Smelt in the proportion of 14.5% to 16% Ni, 7.5% to 8.5% Sn, ≤0.2% Si, 0.3≤% Zn, ≤0.2% Mg, ≤0.3% Mn, ≤0.1% Nb, and the balance is copper, cover with charcoal for protection, and then stand and heat to 1280°C to 1300°C; Nb is added to the holding furnace in the form of CuNb master alloy, and then calcined with charcoal, covered, measured and adjusted, and then sampled for testing;

[0035] 2) Electromagnetic casting: adjust the holding furnace temperature to 1260℃~1280℃, the magnetic field to 30-40HZ, set the normal pulling casting speed to 80mm / min~90mm / min, and after the casting is completed, a copper alloy billet with a diameter of φ195mm is obtained;

[0036] 3) Sawing and segmenting: sawing off 50 mm to 80 mm from the head and tail of the copper alloy bar blank obtained in step 2), and then sawing into 500 mm to 600 mm / segment;

[0037] 4) Homogenization + rapid free forging: The copper alloy bar blank obtained by sawing in step 3) is subjected to high temperature and long-term homogenization at 850°C to 860°C for 8 to 10 hours; rapid free forging is performed in a 1200T rapid forging machine to reduce the extreme temperature loss during the process, ensure that the final forging temperature is greater than 600°C, and obtain a copper alloy bar with a diameter of φ160mm;

[0038] 5) Solution treatment: the copper alloy rod obtained in step 4) is kept at 850° C. to 860° C. for 4 hours, and then rapidly quenched to obtain a supersaturated solution copper alloy rod;

[0039] 6) Precision forging: The bar obtained in step 5) is subjected to high-frequency cold precision forging in a 260T precision forging machine, with the pass processing controlled at 10% to 15% and the total processing deformation of 23%;

[0040] 7) Straightening and sawing: straighten the bars obtained in step 6) and cut them into bars with a length of 90 mm;

[0041] 8) Aging treatment: The bar obtained in step 7) is subjected to aging treatment at 380-400°C for 2.5 hours to strengthen the performance of the copper alloy bar;

[0042] 9) Stress relief annealing: The rod obtained in step 8) is kept at 260-270° C. for 4 hours for stress relief annealing to eliminate the internal stress of the material and obtain a copper alloy rod with maximum strength and plasticity.

[0043] The performance of the Cu-15Ni-8Sn copper alloy rod obtained in this embodiment was tested according to conventional test methods in the industry. The results are shown in Table 1.

[0044] Table 1 Performance test table of Cu-15Ni-8Sn copper alloy rod in the embodiment

[0045]

[0046] Example 2

[0047] A method for preparing a copper alloy rod made of the above-mentioned Cu-15Ni-8Sn copper alloy comprises the following steps:

[0048] 1. A method for preparing an ultra-high-strength Cu15Ni8Sn alloy and a rod thereof for aviation spherical bearings, characterized in that it comprises the following steps:

[0049] 1) Smelting: Smelt in the proportion of 14.5% to 16% Ni, 7.5% to 8.5% Sn, ≤0.2% Si, 0.3≤% Zn, ≤0.2% Mg, ≤0.3% Mn, ≤0.1% Nb, and the balance is copper, cover with charcoal for protection, and then stand and heat to 1280°C to 1300°C; Nb is added to the holding furnace in the form of CuNb master alloy, and then calcined with charcoal, covered, measured and adjusted, and then sampled for testing;

[0050] 2) Electromagnetic casting: adjust the holding furnace temperature to 1260℃~1280℃, the magnetic field to 30-40HZ, set the normal pulling casting speed to 80mm / min~90mm / min, and after the casting is completed, a copper alloy billet with a diameter of φ245mm is obtained;

[0051] 3) Sawing and segmenting: sawing off 50 mm to 80 mm from the head and tail of the copper alloy bar blank obtained in step 2), and then sawing into 500 mm to 600 mm / segment;

[0052] 4) Homogenization + rapid free forging: The copper alloy bar blank obtained by sawing in step 3) is subjected to high temperature and long-term homogenization at 850°C to 860°C for 8 to 10 hours; rapid free forging is performed in a 1200T rapid forging machine to reduce the extreme temperature loss during the process, ensure that the final forging temperature is greater than 600°C, and obtain a copper alloy bar with a diameter of φ160mm;

[0053] 5) Solution treatment: the copper alloy rod obtained in step 4) is kept at 850° C. to 860° C. for 4 hours, and then rapidly quenched to obtain a supersaturated solution copper alloy rod;

[0054] 6) Precision forging: The bar obtained in step 5) is subjected to high-frequency cold precision forging in a 260T precision forging machine, with the pass processing controlled at 10% to 15% and the total processing deformation of 23%;

[0055] 7) Straightening and sawing: straighten the bars obtained in step 6) and cut them into bars with a length of 90 mm;

[0056] 8) Aging treatment: The bar obtained in step 7) is subjected to aging treatment at 380-400°C for 2.5 hours to strengthen the performance of the copper alloy bar;

[0057] 9) Stress relief annealing: The rod obtained in step 8) is kept at 260-270° C. for 4 hours for stress relief annealing to eliminate the internal stress of the material and obtain a copper alloy rod with maximum strength and plasticity.

[0058] The performance of the Cu-15Ni-8Sn copper alloy rod obtained in this example was tested according to conventional test methods in the industry. The results are shown in Table 2.

[0059] Table 2 Performance test table of Cu-15Ni-8Sn copper alloy rod in the embodiment

[0060]

[0061] Example 3

[0062] A method for preparing a copper alloy rod made of the above-mentioned Cu-15Ni-8Sn copper alloy comprises the following steps:

[0063] 1. A method for preparing an ultra-high-strength Cu15Ni8Sn alloy and a rod thereof for aviation spherical bearings, characterized in that it comprises the following steps:

[0064] 1) Smelting: Smelt in the proportion of 14.5% to 16% Ni, 7.5% to 8.5% Sn, ≤0.2% Si, 0.3≤% Zn, ≤0.2% Mg, ≤0.3% Mn, ≤0.1% Nb, and the balance is copper, cover with charcoal for protection, and then stand and heat to 1280°C to 1300°C; Nb is added to the holding furnace in the form of CuNb master alloy, and then calcined with charcoal, covered, measured and adjusted, and then sampled for testing;

[0065] 2) Electromagnetic casting: adjust the holding furnace temperature to 1260℃~1280℃, the magnetic field to 30-40HZ, set the normal pulling casting speed to 80mm / min~90mm / min, and after the casting is completed, a copper alloy billet with a diameter of φ245mm is obtained;

[0066] 3) Sawing and segmenting: sawing off 50 mm to 80 mm from the head and tail of the copper alloy bar blank obtained in step 2), and then sawing into 500 mm to 600 mm / segment;

[0067] 4) Homogenization + rapid free forging: The copper alloy bar blank obtained by sawing in step 3) is subjected to high temperature and long-term homogenization at 850°C to 860°C for 8 to 10 hours; rapid free forging is performed in a 1200T rapid forging machine to reduce the extreme temperature loss during the process, ensure that the final forging temperature is greater than 600°C, and obtain a copper alloy bar with a diameter of φ160mm;

[0068] 5) Solution treatment: the copper alloy rod obtained in step 4) is kept at 850° C. to 860° C. for 4 hours, and then rapidly quenched to obtain a supersaturated solution copper alloy rod;

[0069] 6) Precision forging: The bar obtained in step 5) is subjected to high-frequency cold precision forging in a 260T precision forging machine, with the pass processing controlled at 10% to 15% and the total processing deformation of 38%;

[0070] 7) Straightening and sawing: straighten the bars obtained in step 6) and cut them into bars with a length of 90 mm;

[0071] 8) Aging treatment: The bar obtained in step 7) is subjected to aging treatment at 380-400°C for 2.5 hours to strengthen the performance of the copper alloy bar;

[0072] 9) Stress relief annealing: The rod obtained in step 8) is kept at 260-270° C. for 4 hours for stress relief annealing to eliminate the internal stress of the material and obtain a copper alloy rod with maximum strength and plasticity.

[0073] The performance of the Cu-15Ni-8Sn copper alloy rod obtained in this embodiment was tested according to conventional test methods in the industry. The results are shown in Table 3.

[0074] Table 3 Performance test table of Cu-15Ni-8Sn copper alloy rod in the embodiment

[0075]

[0076] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An ultra-high strength Cu15Ni8Sn alloy for aviation spherical bearings, characterized in that: The invention comprises the following components in mass percentage: 14.5% to 16% Ni, 7.5% to 8.5% Sn, ≤0.2% Si, 0.3≤% Zn, ≤0.2% Mg, ≤0.3% Mn, ≤0.1% Nb, and the balance Cu and unavoidable impurities.

2. A method for preparing an ultra-high strength Cu15Ni8Sn alloy bar for aviation spherical bearings, applied to the ultra-high strength Cu15Ni8Sn alloy for aviation spherical bearings according to claim 1, characterized in that: The specific steps include: Step 1: Smelting: Smelt according to the ratio of 14.5% to 16% Ni, 7.5% to 8.5% Sn, ≤0.2% Si, 0.3≤% Zn, ≤0.2% Mg, ≤0.3% Mn, ≤0.1% Nb, and the balance is copper, add charcoal to cover and protect, then stand and heat to 1280℃~1300℃; Nb is added to the holding furnace in the form of CuNb master alloy, then calcine charcoal to cover, measure and adjust the temperature, and then take samples for testing; Step 2: electromagnetic casting: adjust the temperature of the holding furnace to 1260℃~1280℃, the magnetic field to 30-40HZ, set the normal pulling casting speed to 80mm / min~90mm / min, and after the casting is completed, the copper alloy billet is obtained, and the grain size of the organization is 50~100μm; Step 3: sawing and segmenting: saw off 50mm to 80mm from the head and tail of the copper alloy billet obtained in step 2, and then sawing it into 500mm to 600mm / segment; Step 4: Homogenization + rapid free forging: The copper alloy billet obtained by sawing in step 3 is subjected to high temperature and long-term homogenization at 850℃~860℃ for 8~10h; rapid free forging is performed in a 1200T rapid forging machine to reduce the extreme temperature loss during the process, ensure that the final forging temperature is greater than 600℃, and obtain a copper alloy bar with a diameter and a microstructure grain size of 30~50μm; Step 5: Solution treatment: The copper alloy rod obtained in step 4 is kept at 850°C to 860°C for 4 hours, and then quickly quenched to obtain a supersaturated solution copper alloy rod; Step 6: Precision forging: The bar obtained in step 5 is subjected to high-frequency cold precision forging in a 260T precision forging machine, with the pass processing controlled at 10% to 15% and the total processing deformation less than 40%; Step 7: Straightening and sawing: Straighten the bars obtained in step 6 and cut them into 90mm long bars; Step 8: Aging treatment: The bar obtained in step 7 is subjected to aging treatment at 380-400°C for 2.5 hours to strengthen the performance of the copper alloy bar; Step 9: Stress relief annealing: The rod obtained in step 8 is kept at 260-270°C for 4 hours for stress relief annealing to eliminate the internal stress of the material and obtain the copper alloy rod with maximum strength and plasticity.