Titanium alloy for aviation fastener and preparation method thereof
By adding zirconium tin alloy to aviation fasteners and performing solid solution treatment, the problem of both strength and toughness of titanium alloy is solved, the yield strength and tensile strength of titanium alloy are improved, and the demand for high-performance materials in the aviation industry is met. .
Patent Information
- Application Number
- CN202310584175.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
Existing titanium alloys for aviation fasteners are difficult to combine high strength and good toughness, and cannot meet the increasingly demanding industrial service standards.
By adding zirconium tin alloy as an intermediate alloy and performing solid solution treatment, the yield strength, tensile strength and elongation of the titanium alloy are improved, and the overall strength and toughness are improved.
It significantly improves the yield strength and tensile strength of titanium alloy, controls the pulling deformation amount, enhances the overall strength and toughness of titanium alloy, and meets the high performance requirements of aviation fasteners.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium alloy materials, in particular to a titanium alloy for aviation fasteners and a preparation method thereof. Background Art
[0002] With the acceleration of the replacement of military and civilian aircraft at home and abroad and the continuous improvement of aircraft performance requirements, the conditions for aircraft structural materials have become more stringent, and materials with good comprehensive performance are urgently required. The comprehensive performance of titanium is favored by aircraft designers, and its use in aircraft is constantly increasing. The aviation industry is an important market for titanium alloys. At present, about 3 / 4 of the world's titanium alloys are used in aerospace and military products. Titanium alloys are used to make general structural parts, assemblies and fasteners of aircraft, and even large integral structural parts.
[0003] The existing commonly used titanium alloys for fasteners often cannot have both high strength and good toughness. Structural titanium alloys, with their excellent machinability and mechanical properties, are used in the aerospace industry to manufacture high-strength and complex-shaped parts, such as wing joint structural parts of aircraft, fuselage and landing gear connection frames, hanging engine joints, and other parts, as well as the production of important or key load-bearing parts with high strength and durability requirements. However, as traditional titanium alloys for aviation structures, their combined mechanical properties of strength and toughness are difficult to meet the increasingly stringent industrial service standards, so it is necessary to invent titanium alloys for aviation fasteners and their preparation methods to solve the above problems. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the shortcomings of the prior art, the present invention provides a titanium alloy for aviation fasteners and a preparation method thereof. By adding a zirconium-tin alloy as an intermediate alloy, the yield strength and tensile strength of the produced titanium alloy are improved, and the titanium alloy is subsequently subjected to a solid solution treatment to increase the elongation of the titanium alloy, thereby improving the overall strength and toughness of the titanium alloy. The comprehensive mechanical properties.
[0006] (II) Technical solution
[0007] In order to achieve the above-mentioned improvement of the yield strength and tensile strength of the titanium alloy, and the improvement of the elongation of the titanium alloy, so as to improve the overall strength and toughness comprehensive mechanical properties of the titanium alloy, the present invention provides the following technical solution: a titanium alloy for aviation fasteners, comprising the following raw materials in proportion by weight: barium: 10-15 parts, yttrium: 20-30 parts, aluminum: 40-50 parts, ruthenium: 2-3 parts, osmium: 1-2 parts, germanium: 10-15 parts, zirconium: 10-20 parts, tin: 15-25 parts, vanadium: 35-45 parts, silicon: 1-2 parts, titanium: 65-85 parts.
[0008] Preferably, the titanium element is provided in the form of sponge titanium with a purity of 99.1-99.7%, the aluminum and vanadium elements are provided in the form of an aluminum-vanadium binary alloy containing more than 45% vanadium as an intermediate alloy, and the zirconium and tin elements are provided in the form of a zirconium-tin alloy containing more than 40% zirconium as an intermediate alloy.
[0009] A method for preparing titanium alloy for aviation fasteners comprises the following steps:
[0010] S1. Mix various alloy materials to obtain alloy material bags, and stack titanium sponge and alloy material bags alternately; the titanium sponge is divided into more than 3 layers, and the alloy material bags are divided into more than 3 layers and stacked alternately;
[0011] S2, placing the alloy package prepared in step S1 into a water-cooled copper crucible of a non-consumable vacuum arc furnace, adjusting the position of the tungsten electrode so that the distance between it and the alloy package placed in the water-cooled copper crucible is 0.5 mm to 1.5 mm, closing the furnace door and the vent valve, evacuating to 0.06 Pa to 0.08 Pa, and adjusting the arc current to gradually increase to 250 A to 350 A after arcing until all the raw materials are melted, and cooling to room temperature with the furnace to obtain a titanium alloy ingot;
[0012] S3, repeatedly melting and cooling the titanium alloy ingot obtained in S2 to room temperature in a water-cooled copper crucible to obtain a titanium alloy ingot with relatively uniform composition, and then casting the titanium alloy ingot after the last melting operation. After the titanium alloy is completely cooled, the furnace is opened and the obtained titanium alloy ingot is taken out;
[0013] S4, homogenizing and annealing the titanium alloy ingot obtained in S3 in a vacuum annealing furnace to obtain a cast alloy billet;
[0014] S5, subjecting the as-cast alloy billet obtained in S4 to heat preservation treatment and then deforming the billet to obtain a densified alloy billet;
[0015] S6, subjecting the titanium alloy blank obtained in S5 to a solid solution treatment to obtain a strong and tough titanium alloy;
[0016] S7. The titanium alloy obtained in S6 is straightened by a straightening machine and then polished to ensure a dimensional accuracy of ±0.10 mm and no creases or cracks on the surface, thereby obtaining the aviation fastener.
[0017] Preferably, in step S2, the whole process is protected by high-purity argon gas, and after adding the alloy material package, the vacuum is first evacuated to a vacuum pressure value of >2×10 -2 Pa, and then high-purity argon gas is filled in to a vacuum pressure value of 0.06Pa~0.08Pa.
[0018] Preferably, in step S3, the smelting operation process is performed 4 to 6 times.
[0019] Preferably, in step S4, the vacuum degree in the vacuum annealing furnace is > 2×10-3 Pa, temperature is 950℃~1100℃, and annealing time is 7h~9h.
[0020] Preferably, in step S5, the temperature of the heat preservation treatment is 850-950° C., and the time of the heat preservation treatment is 0.5-1.0 h.
[0021] Preferably, in step S5, the deformation is rolling deformation; the total deformation amount of the rolling deformation is 65-70%, and the temperature of the rolling deformation is 850-950°C.
[0022] Preferably, in step S6, the holding temperature of the solution treatment is 850-950° C., the holding time of the solution treatment is 4-6 min, and the cooling method of the solution treatment is water quenching.
[0023] Preferably, in step S7, the polishing rod needs to be subjected to ultrasonic testing to ensure that there are no internal defects.
[0024] (III) Beneficial effects
[0025] Compared with the prior art, the present invention provides a titanium alloy for aviation fasteners and a preparation method thereof, which has the following beneficial effects:
[0026] 1. The titanium alloy for aviation fasteners and the preparation method thereof improve the yield strength and tensile strength of the produced titanium alloy by adding zirconium-tin alloy as an intermediate alloy, and control the drawing deformation within a reasonable range through rolling deformation.
[0027] 2. The titanium alloy for aviation fasteners and the preparation method thereof produce a titanium alloy with excellent comprehensive performance through subsequent solid solution treatment of the titanium alloy, thereby improving the elongation of the titanium alloy and improving the overall strength, toughness and comprehensive mechanical properties of the titanium alloy. DETAILED DESCRIPTION
[0028] The following will combine the contents in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Embodiment 1:
[0030] The present invention provides a technical solution: a titanium alloy for aviation fasteners comprises the following raw materials in proportion by weight: 10 parts of barium, 20 parts of yttrium, 40 parts of aluminum, 2 parts of ruthenium, 1 part of osmium, 10 parts of germanium, 10 parts of zirconium, 15 parts of tin, 35 parts of vanadium, 1 part of silicon and 65 parts of titanium.
[0031] The titanium element is provided in the form of sponge titanium with a purity of 99.1%, the aluminum and vanadium elements are provided in the form of aluminum-vanadium binary alloy containing 45% vanadium as an intermediate alloy, and the zirconium and tin elements are provided in the form of zirconium-tin alloy containing 40% zirconium as an intermediate alloy.
[0032] A method for preparing titanium alloy for aviation fasteners comprises the following steps:
[0033] S1. Mix various alloy materials to obtain alloy material bags, and stack titanium sponge and alloy material bags alternately; the titanium sponge is divided into 3 layers, and the alloy material bags are divided into 3 layers and stacked alternately;
[0034] S2. Place the alloy package prepared in step S1 into a water-cooled copper crucible in a non-consumable vacuum arc furnace. Adjust the position of the tungsten electrode so that the distance between it and the alloy package in the water-cooled copper crucible is 0.5 mm. Close the furnace door and the vent valve, and evacuate the furnace to a vacuum pressure of 2×10 -2 After the temperature reaches 0.050 Pa, high-purity argon gas is filled in for protection and then vacuumized to 0.06 Pa. After the arc is started, the arc current is gradually increased to 250 A until all the raw materials are melted, and the furnace is cooled to room temperature to obtain a titanium alloy ingot.
[0035] S3, repeatedly melting and cooling the titanium alloy ingot obtained in S2 to room temperature in a water-cooled copper crucible, repeating the melting operation process 4 times, obtaining a titanium alloy ingot with relatively uniform composition, and then casting it after the last melting operation, opening the furnace after the titanium alloy is completely cooled, and taking out the obtained titanium alloy ingot;
[0036] S4, homogenizing and annealing the titanium alloy ingot obtained in S3 in a vacuum annealing furnace, the vacuum degree in the vacuum annealing furnace is 2×10 -3 Pa, temperature 950°C, annealing time 7h, to obtain a cast alloy billet;
[0037] S5, subjecting the as-cast alloy billet obtained in S4 to heat preservation treatment and then deformation, the heat preservation treatment temperature is 850° C., the heat preservation treatment time is 0.5 h, the deformation is rolling deformation, the total deformation amount of the rolling deformation is 65%, the rolling deformation temperature is 850° C. to obtain a densified alloy billet;
[0038] S6, subjecting the titanium alloy blank obtained in S5 to a solid solution treatment, wherein the holding temperature of the solid solution treatment is 850° C., the holding time of the solid solution treatment is 4 min, and the cooling method of the solid solution treatment is water quenching, so as to obtain a strong and tough titanium alloy;
[0039] S7. The titanium alloy obtained in S6 is straightened by a straightening machine and then polished to ensure a dimensional accuracy of ±0.10mm and no creases or cracks on the surface. The polished rod needs to be ultrasonically inspected to ensure that there are no internal defects to obtain aviation fasteners.
[0040] Embodiment 2:
[0041] The present invention provides a technical solution: a titanium alloy for aviation fasteners comprises the following raw materials in proportion by weight: 12 parts of barium, 25 parts of yttrium, 45 parts of aluminum, 2 parts of ruthenium, 1 part of osmium, 12 parts of germanium, 15 parts of zirconium, 20 parts of tin, 40 parts of vanadium, 1 part of silicon and 75 parts of titanium.
[0042] The titanium element is provided in the form of sponge titanium with a purity of 99.1%, the aluminum and vanadium elements are provided in the form of aluminum-vanadium binary alloy containing 55% vanadium as an intermediate alloy, and the zirconium and tin elements are provided in the form of zirconium-tin alloy containing 50% zirconium as an intermediate alloy.
[0043] A method for preparing titanium alloy for aviation fasteners comprises the following steps:
[0044] S1. Mix various alloy materials to obtain alloy material bags, and stack titanium sponge and alloy material bags alternately; the titanium sponge is divided into 4 layers, and the alloy material bags are divided into 4 layers and stacked alternately;
[0045] S2. Place the alloy package prepared in step S1 into the water-cooled copper crucible of the non-consumable vacuum arc furnace. Adjust the position of the tungsten electrode so that the distance between it and the alloy package in the water-cooled copper crucible is 1.0 mm. Close the furnace door and the vent valve, and evacuate the furnace to a vacuum pressure of 2.2×10 -2 After the temperature reaches 0.05 Pa, high-purity argon gas is filled in for protection and then vacuumized to 0.07 Pa. After the arc is started, the arc current is gradually increased to 300 A until all the raw materials are melted. The furnace is cooled to room temperature to obtain a titanium alloy ingot.
[0046] S3, repeatedly melting and cooling the titanium alloy ingot obtained in S2 to room temperature in a water-cooled copper crucible, repeating the melting operation process for 5 times, obtaining a titanium alloy ingot with relatively uniform composition, and then casting it after the last melting operation, opening the furnace after the titanium alloy is completely cooled, and taking out the obtained titanium alloy ingot;
[0047] S4, homogenizing and annealing the titanium alloy ingot obtained in S3 in a vacuum annealing furnace, the vacuum degree in the vacuum annealing furnace is 2.2×10 -3 Pa, temperature 1000℃, annealing time 8h, to obtain the as-cast alloy billet;
[0048] S5, subjecting the as-cast alloy billet obtained in S4 to heat preservation treatment and then deformation, the heat preservation treatment temperature is 900° C., the heat preservation treatment time is 0.7 h, the deformation is rolling deformation, the total deformation amount of the rolling deformation is 67%, the rolling deformation temperature is 900° C. to obtain a densified alloy billet;
[0049] S6, subjecting the titanium alloy blank obtained in S5 to a solid solution treatment, wherein the holding temperature of the solid solution treatment is 900° C., the holding time of the solid solution treatment is 5 min, and the cooling method of the solid solution treatment is water quenching, so as to obtain a strong and tough titanium alloy;
[0050] S7. The titanium alloy obtained in S6 is straightened by a straightening machine and then polished to ensure a dimensional accuracy of ±0.10mm and no creases or cracks on the surface. The polished rod needs to be ultrasonically inspected to ensure that there are no internal defects to obtain aviation fasteners.
[0051] Embodiment 3:
[0052] The present invention provides a technical solution: a titanium alloy for aviation fasteners comprises the following raw materials in proportion by weight: 15 parts of barium, 30 parts of yttrium, 50 parts of aluminum, 3 parts of ruthenium, 2 parts of osmium, 15 parts of germanium, 20 parts of zirconium, 25 parts of tin, 45 parts of vanadium, 2 parts of silicon and 80 parts of titanium.
[0053] The titanium element is provided in the form of sponge titanium with a purity of 99.1%, the aluminum and vanadium elements are provided in the form of aluminum-vanadium binary alloy containing 55% vanadium as an intermediate alloy, and the zirconium and tin elements are provided in the form of zirconium-tin alloy containing 50% zirconium as an intermediate alloy.
[0054] A method for preparing titanium alloy for aviation fasteners comprises the following steps:
[0055] S1. Mix various alloy materials to obtain alloy material bags, and stack titanium sponge and alloy material bags alternately; the titanium sponge is divided into 3 layers, and the alloy material bags are divided into 3 layers and stacked alternately;
[0056] S2. Place the alloy package prepared in step S1 into the water-cooled copper crucible of the non-consumable vacuum arc furnace. Adjust the position of the tungsten electrode so that the distance between it and the alloy package in the water-cooled copper crucible is 1.0 mm. Close the furnace door and the vent valve, and evacuate the furnace to a vacuum pressure of 2.0×10 -2 After the temperature reaches 0.07 Pa, high-purity argon gas is filled for protection and then vacuumized to 0.07 Pa. After the arc is started, the arc current is adjusted to gradually increase to 320 A until all the raw materials are melted, and the furnace is cooled to room temperature to obtain a titanium alloy ingot.
[0057] S3, repeatedly melting and cooling the titanium alloy ingot obtained in S2 to room temperature in a water-cooled copper crucible, repeating the melting operation process 4 times, obtaining a titanium alloy ingot with relatively uniform composition, and then casting it after the last melting operation, opening the furnace after the titanium alloy is completely cooled, and taking out the obtained titanium alloy ingot;
[0058] S4, homogenizing and annealing the titanium alloy ingot obtained in S3 in a vacuum annealing furnace, the vacuum degree in the vacuum annealing furnace is 2.0×10 -3 Pa, temperature 1100°C, annealing time 8.5h, to obtain a cast alloy billet;
[0059] S5, subjecting the cast alloy billet obtained in S4 to heat preservation treatment and then deforming, wherein the temperature of the heat preservation treatment is 900° C., the time of the heat preservation treatment is 1.0 h, the deformation is rolling deformation, the total deformation amount of the rolling deformation is 67%, and the temperature of the rolling deformation is 900° C. to obtain a densified alloy billet;
[0060] S6, subjecting the titanium alloy blank obtained in S5 to a solid solution treatment, wherein the holding temperature of the solid solution treatment is 900° C., the holding time of the solid solution treatment is 6 min, and the cooling method of the solid solution treatment is water quenching, so as to obtain a strong and tough titanium alloy;
[0061] S7. The titanium alloy obtained in S6 is straightened by a straightening machine and then polished to ensure a dimensional accuracy of ±0.10mm and no creases or cracks on the surface. The polished rod needs to be ultrasonically inspected to ensure that there are no internal defects to obtain aviation fasteners.
[0062] Embodiment 4:
[0063] The present invention provides a technical solution: a titanium alloy for aviation fasteners comprises the following raw materials in proportion by weight: 15 parts of barium, 30 parts of yttrium, 50 parts of aluminum, 3 parts of ruthenium, 2 parts of osmium, 15 parts of germanium, 20 parts of zirconium, 25 parts of tin, 45 parts of vanadium, 2 parts of silicon and 85 parts of titanium.
[0064] The titanium element is provided in the form of sponge titanium with a purity of 99.7%, the aluminum and vanadium elements are provided in the form of aluminum-vanadium binary alloy containing 50% vanadium as an intermediate alloy, and the zirconium and tin elements are provided in the form of zirconium-tin alloy containing 50% zirconium as an intermediate alloy.
[0065] A method for preparing titanium alloy for aviation fasteners comprises the following steps:
[0066] S1. Mix various alloy materials to obtain alloy material bags, and stack titanium sponge and alloy material bags alternately; the titanium sponge is divided into 4 layers, and the alloy material bags are divided into 4 layers and stacked alternately;
[0067] S2. Place the alloy package prepared in step S1 into the water-cooled copper crucible of the non-consumable vacuum arc furnace. Adjust the position of the tungsten electrode so that the distance between it and the alloy package in the water-cooled copper crucible is 1.5 mm. Close the furnace door and the vent valve, and evacuate the furnace to a vacuum pressure of 2.5×10 -2 After the furnace reaches 0.05 Pa, high-purity argon gas is filled in for protection and then vacuumized to 0.08 Pa. After the arc is started, the arc current is gradually increased to 350 A until all the raw materials are melted, and the furnace is cooled to room temperature to obtain a titanium alloy ingot.
[0068] S3, repeatedly melting and cooling the titanium alloy ingot obtained in S2 to room temperature in a water-cooled copper crucible, repeating the melting operation process for 5 times, obtaining a titanium alloy ingot with relatively uniform composition, and then casting it after the last melting operation, opening the furnace after the titanium alloy is completely cooled, and taking out the obtained titanium alloy ingot;
[0069] S4, homogenizing and annealing the titanium alloy ingot obtained in S3 in a vacuum annealing furnace, the vacuum degree in the vacuum annealing furnace is 2.5×10 -3 Pa, temperature 1100°C, annealing time 9h, to obtain a cast alloy billet;
[0070] S5, subjecting the as-cast alloy billet obtained in S4 to heat preservation treatment and then deformation, the heat preservation treatment temperature is 950° C., the heat preservation treatment time is 1.0 h, the deformation is rolling deformation, the total deformation amount of the rolling deformation is 70%, and the rolling deformation temperature is 950° C. to obtain a densified alloy billet;
[0071] S6, subjecting the titanium alloy blank obtained in S5 to a solid solution treatment, wherein the holding temperature of the solid solution treatment is 950° C., the holding time of the solid solution treatment is 6 min, and the cooling method of the solid solution treatment is water quenching, so as to obtain a strong and tough titanium alloy;
[0072] S7. The titanium alloy obtained in S6 is straightened by a straightening machine and then polished to ensure a dimensional accuracy of ±0.10mm and no creases or cracks on the surface. The polished rod needs to be ultrasonically inspected to ensure that there are no internal defects to obtain aviation fasteners.
[0073] The titanium alloy for aviation fasteners and the preparation method thereof improve the yield strength and tensile strength of the produced titanium alloy by adding a zirconium-tin alloy as an intermediate alloy, control the drawing deformation within a reasonable range through rolling deformation, and produce a titanium alloy with excellent comprehensive performance by subsequent solid solution treatment of the titanium alloy, thereby improving the elongation of the titanium alloy and improving the overall strength, toughness and comprehensive mechanical properties of the titanium alloy.
[0074] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. Titanium alloy for aviation fasteners, characterized in that: The invention comprises the following raw materials in proportion by weight: barium: 10-15 parts, yttrium: 20-30 parts, aluminum: 40-50 parts, ruthenium: 2-3 parts, osmium: 1-2 parts, germanium: 10-15 parts, zirconium: 10-20 parts, tin: 15-25 parts, vanadium: 35-45 parts, silicon: 1-2 parts, and titanium: 65-85 parts.
2. The titanium alloy for aviation fasteners according to claim 1, characterized in that: The titanium element is provided as a raw material of sponge titanium with a purity of 99.1-99.7%, the aluminum and vanadium elements are provided as an aluminum-vanadium binary alloy containing more than 45% vanadium as an intermediate alloy, and the zirconium and tin elements are provided as a zirconium-tin alloy containing more than 40% zirconium as an intermediate alloy.
3. A method for preparing titanium alloy for aviation fasteners, characterized in that: The following steps are involved: S1. Mix various alloy materials to obtain alloy material bags, and stack titanium sponge and alloy material bags alternately; the titanium sponge is divided into more than 3 layers, and the alloy material bags are divided into more than 3 layers and stacked alternately; S2, placing the alloy package prepared in step S1 into a water-cooled copper crucible of a non-consumable vacuum arc furnace, adjusting the position of the tungsten electrode so that the distance between it and the alloy package placed in the water-cooled copper crucible is 0.5 mm to 1.5 mm, closing the furnace door and the vent valve, evacuating to 0.06 Pa to 0.08 Pa, and adjusting the arc current to gradually increase to 250 A to 350 A after arcing until all the raw materials are melted, and cooling to room temperature with the furnace to obtain a titanium alloy ingot; S3, repeatedly melting and cooling the titanium alloy ingot obtained in S2 to room temperature in a water-cooled copper crucible to obtain a titanium alloy ingot with relatively uniform composition, and then casting the titanium alloy ingot after the last melting operation. After the titanium alloy is completely cooled, the furnace is opened and the obtained titanium alloy ingot is taken out; S4, homogenizing and annealing the titanium alloy ingot obtained in S3 in a vacuum annealing furnace to obtain a cast alloy billet; S5, subjecting the as-cast alloy billet obtained in S4 to heat preservation treatment and then deforming the billet to obtain a densified alloy billet; S6, subjecting the titanium alloy blank obtained in S5 to a solid solution treatment to obtain a strong and tough titanium alloy; S7. The titanium alloy obtained in S6 is straightened by a straightening machine and then polished to ensure a dimensional accuracy of ±0.10 mm and no creases or cracks on the surface, thereby obtaining the aviation fastener.
4. The method for preparing titanium alloy for aviation fasteners according to claim 3, characterized in that: In step S2, the whole process is protected by high-purity argon gas. After adding the alloy material package, the vacuum is first evacuated to a vacuum pressure value of >2×10 -2 Pa, and then high-purity argon gas is filled in to a vacuum pressure value of 0.06Pa~0.08Pa.
5. The method for preparing titanium alloy for aviation fasteners according to claim 3, characterized in that: In step S3, the smelting operation process is performed 4 to 6 times.
6. The titanium alloy for aviation fasteners and the preparation method thereof according to claim 2, characterized in that: In step S4, the vacuum degree in the vacuum annealing furnace is > 2×10 -3 Pa, temperature is 950℃~1100℃, and annealing time is 7h~9h.
7. The method for preparing titanium alloy for aviation fasteners according to claim 3, characterized in that: In the step S5, the temperature of the heat preservation treatment is 850-950° C., and the time of the heat preservation treatment is 0.5-1.0 h.
8. The method for preparing titanium alloy for aviation fasteners according to claim 3, characterized in that: In step S5, the deformation is rolling deformation; the total deformation amount of the rolling deformation is 65-70%, and the temperature of the rolling deformation is 850-950°C.
9. The method for preparing titanium alloy for aviation fasteners according to claim 3, characterized in that: In the step S6, the holding temperature of the solution treatment is 850-950° C., the holding time of the solution treatment is 4-6 min, and the cooling method of the solution treatment is water quenching.
10. The method for preparing titanium alloy for aviation fasteners according to claim 3, characterized in that: In step S7, the polished rod needs to be subjected to ultrasonic testing to ensure that there are no internal defects.