Hard alloy for cutting tool and preparation method thereof

By adopting a three-phase cemented carbide, combined with discharge plasma sintering and pressure sintering, using Co powder composite nanozirconia and vanoxa as a result, the problem of decreasing bond strength of WC-based alloys at high temperatures was solved, and the hardness was significantly improved Mechanical properties and chemical stability of alloys.

CN119020653APending Publication Date: 2024-11-26YONGCHENG MEIZHU (BEIJING) CONSTRUCTION TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411152389.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The bonding strength of the existing tungsten carbide (WC)-based carbide has decreased under high temperature environments, resulting in a shortening of service life. Although Co as a bonding phase material improves toughness, it reduces the hardness and oxidation resistance of the alloy.

Method used

Carbides with three-phase structure, including WC grains, carbon solid solution and Co powder composite nanozirconia, were prepared by discharge plasma sintering and pressure sintering. Vanadium oxalate was used as an inhibitor to control grain growth and improve bonding. strength.

Benefits of technology

It significantly improves the mechanical properties, hardness and high-temperature chemical stability of cemented carbide, enhances impact resistance and fracture toughness, and extends service life.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a hard alloy for a cutting tool and a preparation method thereof, and relates to the field of hard alloys. The alloy structure comprises an alpha phase, a beta phase and a gamma phase. The alpha phase is WC grains, and the beta phase is a carbon solid solution; and the gamma phase is Co powder composite nano zirconium oxide. According to the method, Co powder composite nano zirconium oxide is used as a binding phase, a carbon solid solution is mixed in WC grains to serve as a hard phase, vanadyl oxalate is used as an inhibitor, a sintered preform is prepared through a spark plasma sintering method, and then the hard alloy is obtained through a pressure sintering method. The coarse alpha phase in the three-phase structure is beneficial for increasing the average free path of the binding phase and improving the strength and toughness of the alloy, the fine particle beta phase is good in chemical stability, meanwhile, the synergistic effect of the binding phase, the nano zirconium oxide and Co is strengthened, the binding phase is evenly distributed, the fracture toughness is improved, and the inhibitor prevents grain growth during forming. The prepared hard alloy is highly densified, uniform in density, high in hardness and plastic deformation resistance and stable in chemical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cemented carbide, in particular to a cemented carbide for cutting tools and a preparation method thereof. Background Art

[0002] Cemented carbide is a composite material composed of a refractory hard phase and a metal bonding phase. It is widely used in the fields of automobiles, aerospace, oil exploration, mining, mechanical processing, etc. The most widely used metal bonding phase material for tungsten carbide (WC)-based cemented carbide is cobalt (Co). Co has excellent wettability and high yield strength to WC, which gives cemented carbide excellent mechanical properties. Although Co as a bonding phase material can improve the toughness of the alloy, it will reduce the hardness, oxidation resistance and corrosion resistance of the alloy. Especially in high temperature environments, WC is easy to detach from Co, the bonding strength decreases, and the service life of the alloy is reduced.

[0003] Nano-oxide ceramics are advanced ceramic materials with nanoscale grains. They usually exhibit better performance than traditional ceramics and have potential applications in many fields, such as aerospace, nuclear energy, high-temperature structural materials, thermal protection systems, and energy conservation and environmental protection. For example, the research team of Donghua University has developed a new phase change modulation strategy. By controlling the grain growth of oxide ceramic nanofibers at high temperatures, it has achieved effective regulation of the morphology and size uniformity of the primary grains, thereby inhibiting the malignant growth of the grains. The use of nano-oxide ceramics to prepare cemented carbide is an innovative method aimed at improving the performance of cemented carbide and reducing production costs. Summary of the invention

[0004] The object of the present invention is to provide a cemented carbide for cutting tools and a preparation method thereof, so as to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a cemented carbide for cutting tools, the cemented carbide for cutting tools contains three phases: α phase, β phase and γ phase; the α phase is WC grains, the β phase is a carbon solid solution, and the γ phase is Co powder composite nano-zirconia; the α phase and β phase are hard phases, and the γ phase is a bonding phase; the cemented carbide includes the following components by weight: 67 to 75 parts of α phase, 6 to 10 parts of β phase, 8 to 15 parts of γ phase, and 1 to 3 parts of inhibitor vanadyl oxalate; the cemented carbide is prepared by mixing β phase into α phase, adding Co powder and nano-zirconia, adding inhibitor, ball milling, and then by spark plasma sintering and pressure sintering.

[0006] Furthermore, the average grain size of the α phase is 2.0-4.0 μm; the average grain size of the β phase is 1-2 μm.

[0007] Furthermore, the mass proportions of the raw materials of the β-phase carbon solid solution are: 40-50 parts of solid carbon source powder, 40-45 parts of W source powder, 3-4 parts of Ti source powder, and 0.5-1.5 parts of Ta source powder.

[0008] Furthermore, the β-phase carbon solid solution is prepared by the following method:

[0009] (1) putting Ti source powder, W source powder, Ta source powder and solid carbon source powder into a ball mill container, adding ball milling medium and forming agent to perform ball milling and mixing;

[0010] (2) placing the ball milled and mixed liquid into a spray granulation device for spray granulation, spray granulation can form uniform particles, and then dry and dehydrate;

[0011] (3) The dried pellets are placed in a high-temperature carbonization furnace, maintained at high temperature, and reacted completely under inert gas to prepare a β-phase carbon solid solution powder.

[0012] Further, the vanadyl oxalate is prepared by the following steps:

[0013] (1) dissolving ammonium metavanadate in hot water, filtering at high temperature, and adding carbon black before cooling the filtrate;

[0014] (2) cooling the obtained mixed solution to crystallize while continuously stirring; then performing solid-liquid separation, and reducing and decomposing the obtained heated solid;

[0015] (3) dissolving the obtained product and oxalic acid in hot water, cooling the obtained mixed solution, placing it in a container containing vanadyl oxalate seed crystals, and allowing it to stand for crystallization; and then performing solid-liquid separation to obtain high-purity vanadyl oxalate crystals.

[0016] Furthermore, the nano zirconium oxide is prepared by the following steps:

[0017] (1) mixing zirconium salt, citric acid and ammonium chloride solution to obtain a mixed solution;

[0018] (2) adding ammonia water dropwise to the obtained mixed solution to perform a precipitation reaction to obtain Zr(OH)4 colloid;

[0019] (3) Zr(OH )4 The colloid is aged, washed with water and washed with alcohol in sequence to obtain hydrated zirconium gel, which is then dried to obtain a zirconium precursor; the obtained zirconium precursor is calcined to obtain nano zirconium oxide.

[0020] Furthermore, a method for preparing a cemented carbide for a cutting tool comprises the following preparation steps:

[0021] (1) Pre-wet grinding the carbon solid solution powder in a ball mill, and then wet grinding it together with WC grains, Co powder, nano zirconium oxide, and vanadyl oxalate in a ball mill under an inert gas atmosphere, and drying after wet grinding;

[0022] (2) placing the dried mixture in a spark plasma sintering furnace for spark plasma sintering in an inert gas atmosphere to obtain a cemented carbide pre-sintered body;

[0023] (3) The cemented carbide pre-sintered body is placed in a special reaction furnace for pressure sintering, vacuum sintered, and cooled to form a cemented carbide for cutting tools.

[0024] Furthermore, the inert gas is argon; and the vacuum pressure is 30-45 MPa.

[0025] Furthermore, in the spark plasma sintering method, the current is maintained at 500-2000A and the voltage is maintained at 20-50V;

[0026] Furthermore, in the spark plasma sintering, the temperature is first raised to 800-810°C, and sintered at this temperature for 1-2 minutes, and then the temperature is further raised to 1200-1300°C, and sintered at this temperature for 3-6 minutes; in the pressure sintering, the temperature is 1200-1350°C, and the sintering time is 1-2 hours.

[0027] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0028] The present invention prepares cemented carbide through a three-phase structure, uses Co composite nano-zirconia as a bonding metal γ phase, and uses α phase (WC grains) and β phase [carbon solid solution (Ti, W, Ta)] as hard phases. The relatively coarse α phase in the three-phase structure is beneficial to increasing the mean free path of the bonding phase and improving the toughness of the alloy, while the fine particle β phase has good high-temperature chemical stability and can disperse and strengthen the bonding phase, thereby improving the hardness and plastic deformation resistance of the alloy, so that while the alloy maintains high strength and good impact resistance, its high hardness, high temperature resistance and excellent chemical stability are also significantly improved.

[0029] The nano zirconium oxide and metal Co prepared by the sol-gel method are used as a composite bonding phase. The nano zirconium oxide has good thermodynamic compatibility with metal WC and can be evenly distributed between WC crystal grain matrices during sintering. During sintering, the WC crystal grains retain the initial grain size. The even distribution of the bonding phase limits the grain boundary mobility and significantly inhibits the grain growth of the WC matrix. After sintering, it can achieve nearly complete densification and significantly improve the mechanical properties of the cemented carbide. In addition, the stress-induced phase transformation of the nano zirconium oxide, such as the transformation from the tetragonal phase to the monoclinic phase, can absorb energy during the process and synergize with CO to improve the fracture toughness of the cemented carbide.

[0030] The present invention uses vanadyl oxalate as an inhibitor. During the wet grinding process, the vanadyl oxalate is dissolved in the grinding liquid, and the dispersion effect is remarkable. Vanadium is evenly distributed in the slurry in an ionic state, and is precipitated and adsorbed on the surface of WC and other particles during the drying process. During the sintering process, the vanadyl oxalate is decomposed and finally in-situ reduced and carbonized to nano-vanadium carbide, which is evenly distributed in the entire alloy, inhibiting the growth of grains and improving the performance of cemented carbide.

[0031] A cemented carbide for cutting tools prepared by the present invention is fixed and formed by combining a discharge plasma sintering method and a pressure sintering method. A discharge plasma sintering process is first used to form a pre-sintered body. This method has a short sintering time and can retain the fine microstructure left in the ball milling process, so that the material has good mechanical properties. The sintering speed is fast, and the degree of element diffusion in this process is low. While inhibiting the growth of grains, the added superhard material matrix is ​​better retained in the matrix, greatly improving the hardness of the material. Then, the pressure sintering method is used to complete full densification, eliminate the residual pores inside the alloy to the maximum extent, improve the density and uniformity of the alloy, and thus significantly improve the physical and mechanical properties of the cemented carbide. DETAILED DESCRIPTION

[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the cemented carbide for cutting tools prepared in the following examples are as follows:

[0034] Bending strength: Select a 40mm×20mm×3mm cemented carbide sample and test the bending strength according to GB / T232-2024;

[0035] Hardness: Select a 40mm×20mm×3mm cemented carbide sample and test the hardness according to GB / T230.1-2018;

[0036] Porosity: Select a 40mm×20mm×3mm cemented carbide sample and test the porosity according to GB / T3489-2015;

[0037] Example 1

[0038] (1) 3.5 parts of Ti source powder, 42.5 parts of W source powder, 1 part of Ta source powder and 45 parts of solid carbon source powder were placed in a ball mill container, tungsten carbide balls were added as ball milling media with a medium filling rate of 45%, and 2 parts of polyethylene glycol was used as a molding agent for ball milling and mixing for 15 hours;

[0039] (2) placing the mixed liquid after ball milling into a spray granulation device for spray granulation to form uniform particles, and drying and dehydrating;

[0040] (3) The dried pellets were placed in a high-temperature carbonization furnace and reacted at 1650° C. in an argon-containing mixed reducing atmosphere for 2.5 h to prepare a β-phase carbon solid solution powder.

[0041] (4) dissolving 10 parts of ammonium metavanadate in hot water at 90°C, maintaining the high temperature at 90°C, filtering, and adding 2 parts of carbon black before cooling the filtrate;

[0042] (5) cooling the mixed solution obtained in step (4) at 30° C. for crystallization, and continuously stirring at a rate of 100 r / min for 6 h; then performing solid-liquid separation, heating to 500° C., reacting for 1.5 h, and reducing and decomposing the solid;

[0043] (6) The product obtained in step (5) and 12 parts of oxalic acid are dissolved in hot water at 85° C. After the obtained mixed solution is cooled to room temperature, it is placed in a container containing 1.5 parts of vanadyl oxalate seed crystals for standing and crystallization; and then solid-liquid separation is performed to obtain high-purity vanadyl oxalate crystals.

[0044] (7) 25 parts of ZrCl4, 2 parts of citric acid, and 20 parts of ammonium chloride with a concentration of 6.6 mol / L were mixed to obtain a mixed solution;

[0045] (8) adding 100 parts by mass of 30% ammonia water dropwise to the mixed solution obtained in step (7) to carry out a precipitation reaction to obtain Zr(OH)4 colloid;

[0046] (9) The Zr(OH)4 colloid is aged, washed with water and washed with alcohol in sequence, and the temperature is maintained at 50°C during the process to obtain a hydrated zirconium gel, which is then dried to obtain a zirconium precursor; the obtained zirconium precursor is calcined at 800°C for 2h to obtain nano zirconium oxide.

[0047] (10) 8 parts of carbon solid solution powder were pre-wet-milled in a ball mill for 14 h, and then wet-milled together with 71 parts of WC grains, 8 parts of Co powder, 4 parts of nano zirconium oxide, and 2 parts of vanadyl oxalate in a ball mill for 21 h under an argon atmosphere, and dried after wet milling;

[0048] (11) placing the dried mixture in a spark plasma sintering furnace for spark plasma sintering in an argon atmosphere, heating to 805° C., sintering at this temperature for 1.5 min, and then heating to 1250° C., sintering at this temperature for 4.5 min to obtain a cemented carbide pre-sintered body;

[0049] (12) The cemented carbide pre-sintered body is placed in a special reaction furnace for pressure sintering, evacuated to maintain the pressure at 37.5 MPa, maintained at a temperature of 1275° C., sintered for 1.5 h, molded and cooled, to obtain a cemented carbide for cutting tools.

[0050] Example 2

[0051] (1) 4 parts of Ti source powder, 45 parts of W source powder, 1.5 parts of Ta source powder and 50 parts of solid carbon source powder were placed in a ball mill container, tungsten carbide balls were added as ball milling media with a medium filling rate of 50%, and 3 parts of polyethylene glycol was used as a molding agent for ball milling and mixing for 18 hours;

[0052] (2) placing the mixed liquid after ball milling into a spray granulation device for spray granulation to form uniform particles, and drying and dehydrating;

[0053] (3) The dried pellets are placed in a high-temperature carbonization furnace and reacted at 1900° C. in an argon-containing mixed reducing atmosphere for 3 hours to prepare a β-phase carbon solid solution powder.

[0054] (4) dissolving 12 parts of ammonium metavanadate in hot water at 95°C, maintaining the high temperature at 95°C, filtering, and adding 3 parts of carbon black before cooling the filtrate;

[0055] (5) cooling the mixed solution obtained in step (4) at 35° C. to crystallize, and continuously stirring at a rate of 120 r / min for 8 h; then performing solid-liquid separation, heating to 550° C., reacting for 2 h, and reducing and decomposing the solid;

[0056] (6) The product obtained in step (5) and 16 parts of oxalic acid are dissolved in hot water at 90° C. After the obtained mixed solution is cooled to room temperature, it is placed in a container containing 2 parts of vanadyl oxalate seed crystals for standing and crystallization; and then solid-liquid separation is performed to obtain high-purity vanadyl oxalate crystals.

[0057] (7) 30 parts of ZrCl4, 3 parts of citric acid, and 25 parts of 6.6 mol / L ammonium chloride were mixed to obtain a mixed solution;

[0058] (8) adding 125 parts by mass of 30% ammonia water dropwise to the mixed solution obtained in step (7) to carry out a precipitation reaction to obtain Zr(OH)4 colloid;

[0059] (9) The Zr(OH)4 colloid is aged, washed with water and washed with alcohol in sequence, while the temperature is maintained at 55°C, to obtain a hydrated zirconium gel, which is then dried to obtain a zirconium precursor; the obtained zirconium precursor is calcined at 1000°C for 3h to obtain nano zirconium oxide.

[0060] (10) 10 parts of carbon solid solution powder were pre-wet-milled in a ball mill for 16 h, and then wet-milled together with 75 parts of WC grains, 10 parts of Co powder, 5 parts of nano zirconium oxide, and 3 parts of vanadyl oxalate in a ball mill for 24 h under an argon atmosphere, and dried after wet milling;

[0061] (11) placing the dried mixture in a spark plasma sintering furnace for spark plasma sintering, heating the mixture to 810° C. in an argon atmosphere, sintering the mixture at a temperature of 2 min, and then heating the mixture to 1300° C. and sintering the mixture at a temperature of 6 min to obtain a cemented carbide pre-sintered body;

[0062] (12) The cemented carbide pre-sintered body is placed in a special reaction furnace for pressure sintering, evacuated to maintain a pressure of 45 MPa, maintained at a temperature of 1350° C., sintered for 2 h, molded and cooled, to obtain a cemented carbide for cutting tools.

[0063] Example 3

[0064] (1) 3 parts of Ti source powder, 40 parts of W source powder, 0.5 parts of Ta source powder and 40 parts of solid carbon source powder were placed in a ball mill container, tungsten carbide balls were added as ball milling media with a medium filling rate of 40%, and 1 part of polyethylene glycol was used as a molding agent for ball milling and mixing for 12 hours;

[0065] (2) placing the mixed liquid after ball milling into a spray granulation device for spray granulation to form uniform particles, and drying and dehydrating;

[0066] (3) The dried pellets are placed in a high-temperature carbonization furnace and reacted for 2 hours at 1400° C. in an argon-containing mixed reducing atmosphere to prepare a β-phase carbon solid solution powder.

[0067] (4) dissolving 10 parts of ammonium metavanadate in hot water at 85°C, maintaining the high temperature at 85°C, filtering, and adding 1 part of carbon black before cooling the filtrate;

[0068] (5) cooling the mixed solution obtained in step (4) at 25° C. for crystallization, and continuously stirring at a rate of 80 r / min for 4 h; then performing solid-liquid separation, heating to 450° C., reacting for 1 h, and reducing and decomposing the solid;

[0069] (6) The product obtained in step (5) and 8 parts of oxalic acid are dissolved in 80° C. hot water. After the obtained mixed solution is cooled to room temperature, it is placed in a container containing 0.5 parts of vanadyl oxalate seed crystals for standing and crystallization; and then solid-liquid separation is performed to obtain high-purity vanadyl oxalate crystals.

[0070] (7) 30 parts of ZrCl4, 3 parts of citric acid, and 25 parts of 6.6 mol / L ammonium chloride were mixed to obtain a mixed solution;

[0071] (8) adding 80 parts by mass of 30% ammonia water dropwise to the mixed solution obtained in step (7) to carry out a precipitation reaction to obtain Zr(OH)4 colloid;

[0072] (9) The Zr(OH)4 colloid is aged, washed with water and washed with alcohol in sequence, and the temperature is maintained at 45°C during the process to obtain a hydrated zirconium gel, which is then dried to obtain a zirconium precursor; the obtained zirconium precursor is calcined at 600°C for 1 hour to obtain nano zirconium oxide.

[0073] (10) 6 parts of carbon solid solution powder were pre-wet-milled in a ball mill for 12 h, and then wet-milled together with 67 parts of WC grains, 6 parts of Co powder, 3 parts of nano zirconium oxide, and 1 part of vanadyl oxalate in a ball mill for 18 h under an argon atmosphere, and dried after wet milling;

[0074] (11) placing the dried mixture in a spark plasma sintering furnace for spark plasma sintering in an argon atmosphere, heating to 800° C., sintering at this temperature for 1 min, and then heating to 1200° C., sintering at this temperature for 3 min to obtain a cemented carbide pre-sintered body;

[0075] (12) The cemented carbide pre-sintered body is placed in a special reaction furnace for pressure sintering, evacuated to maintain the pressure at 30 MPa, maintained at a temperature of 1200° C., sintered for 1 hour, molded and cooled, to obtain a cemented carbide for cutting tools.

[0076] Comparative Example 1

[0077] The difference between Comparative Example 1 and Example 1 is that steps (1), (2) and (3) are deleted, and step (10) is changed to wet grinding 71 parts of WC grains, 8 parts of Co powder, 4 parts of nano zirconium oxide and 2 parts of vanadium oxalate in a ball mill for 21 hours under an argon atmosphere and drying after wet grinding; the remaining steps are the same as those in Example 1.

[0078] Comparative Example 2

[0079] The difference between Comparative Example 2 and Example 1 is that steps (7) to (9) are deleted, and step (10) is changed to first wet-grinding 8 parts of carbon solid solution powder in a ball mill for 14 hours, and then wet-grinding it with 71 parts of WC grains and 12 parts of Co metal powder in a ball mill for 21 hours under an argon atmosphere, and drying after wet grinding; the remaining steps are the same as in Example 1.

[0080] Comparative Example 3

[0081] The difference between Comparative Example 3 and Example 1 is that step (11) is deleted and step (12) is changed to placing the dried mixture in a special reaction furnace for pressure sintering, evacuating to maintain the pressure at 37.5 MPa, maintaining the temperature at 1275°C, sintering for 1.5 hours, forming and cooling to obtain a cemented carbide for cutting tools; the remaining steps are the same as Example 1.

[0082] Comparative Example 4

[0083] The difference between Comparative Example 4 and Example 1 is that steps (4) to (6) are deleted and step (10) is changed to 71 parts of WC grains, 8 parts of Co powder, and 4 parts of nano-zirconium oxide, which are placed in a ball mill container, ball milled and mixed for 12 hours under an argon atmosphere, and dried to obtain a ball milled mixture; the remaining steps are the same as in Example 1.

[0084] Effect example

[0085] Table 1 below shows the performance analysis results of the cemented carbides for cutting tools using Examples 1 to 3 of the present invention and Comparative Examples 1 to 4.

[0086] Table 1

[0087] Bending strength / MPa Hardness / HRA Porosity Example 1 2165 92.2 A02B00 Example 2 2057 89.6 A02B00 Example 3 2105 90.3 A02B00 Comparative Example 1 1957 87.3 A02B00 Comparative Example 2 1853 85.9 A03B00 Comparative Example 3 1896 86.3 A04B00 Comparative Example 4 1947 82.4 A03B00

[0088] From the data comparison of the comparative examples, it can be found that the present invention uses Co powder composite nano-zirconia as a bonding phase, carbon solid solution is mixed into WC grains as a hard phase, and vanadyl oxalate is used as an inhibitor. A sintered preform is first prepared by a discharge plasma sintering method, and then a hard alloy is obtained by a pressure sintering method. The coarser α phase in the three-phase structure is conducive to increasing the mean free path of the bonding phase, improving the toughness of the alloy, and the chemical stability of the fine particle β phase is good. At the same time, the bonding phase is strengthened, and the nano-zirconia and Co act synergistically to make the bonding phase uniformly distributed, improve fracture toughness, and the inhibitor prevents grain growth during forming; first, discharge ion sintering is used, and this method has a fast sintering speed, and the degree of element diffusion in this process is low. While inhibiting the growth of grains, the added superhard material matrix is ​​better retained in the matrix, greatly improving the hardness of the material, and retaining the fine microstructure left in the ball milling process, so that the material has good mechanical properties, which is convenient for subsequent pressure sintering to form a densified hard alloy.

[0089] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A cemented carbide for cutting tools, characterized in that: The cemented carbide for cutting tools contains three phases: α phase, β phase and γ phase; the α phase is WC grains, the β phase is carbon solid solution, and the γ phase is Co powder composite nano zirconium oxide; the α phase and β phase are hard phases, and the γ phase is a bonding phase; the cemented carbide includes the following components by weight: 67-75 parts of α phase, 6-10 parts of β phase, 8-15 parts of γ phase, and 1-3 parts of inhibitor vanadyl oxalate; the cemented carbide is prepared by mixing β phase into α phase, adding Co powder and nano zirconium oxide, adding inhibitor, ball milling, and then using spark plasma sintering and pressure sintering.

2. A cemented carbide for cutting tools according to claim 1, characterized in that: The average grain size of the α phase is 2.0-4.0 μm; the average grain size of the β phase is 1-2 μm.

3. The cemented carbide for cutting tool according to claim 1, characterized in that: The mass proportions of the raw materials of the β-phase carbon solid solution are: 40-50 parts of solid carbon source powder, 40-45 parts of W source powder, 3-4 parts of Ti source powder, and 0.5-1.5 parts of Ta source powder.

4. The cemented carbide for cutting tool according to claim 1, characterized in that: The β-phase carbon solid solution is prepared by the following method: (1) putting Ti source powder, W source powder, Ta source powder and solid carbon source powder into a ball mill container, adding ball milling medium and forming agent to perform ball milling and mixing; (2) placing the mixed liquid after ball milling into a spray granulation device for spray granulation to form uniform particles, and drying and dehydrating; (3) The dried pellets are placed in a high-temperature carbonization furnace, maintained at high temperature, and reacted completely under inert gas to prepare a β-phase carbon solid solution powder.

5. The cemented carbide for cutting tool according to claim 1, characterized in that: The vanadyl oxalate is prepared by the following steps: (1) dissolving ammonium metavanadate in hot water, filtering at high temperature, and adding carbon black before cooling the filtrate; (2) cooling the obtained mixed solution for crystallization while continuously stirring; Then, solid-liquid separation is performed, and the obtained heated solid is reduced and decomposed; (3) dissolving the obtained product and oxalic acid in hot water, cooling the obtained mixed solution, placing it in a container containing vanadyl oxalate seed crystals, and allowing it to stand for crystallization; and then performing solid-liquid separation to obtain high-purity vanadyl oxalate crystals.

6. The cemented carbide for cutting tool according to claim 1, characterized in that: The nano zirconium oxide is prepared by the following steps: (1) mixing zirconium salt, citric acid and ammonium chloride to obtain a mixed solution; (2) adding ammonia water dropwise to the obtained mixed solution to perform a precipitation reaction to obtain Zr(OH)4 colloid; (3) The Zr(OH)4 colloid is aged, washed with water and washed with alcohol in sequence to obtain a hydrated zirconium gel, which is then dried to obtain a zirconium precursor; the obtained zirconium precursor is calcined to obtain nano zirconium oxide.

7. A method for preparing a cemented carbide for cutting tools according to any one of claims 1 to 6, characterized in that: The method comprises the following preparation steps: (1) Pre-wet-grinding the carbon solid solution powder in a ball mill, and then wet-grinding it together with WC grains, Co powder, nano zirconium oxide, and vanadyl oxalate in a ball mill under an inert gas atmosphere, followed by drying; (2) placing the dried mixture in a spark plasma sintering furnace for spark plasma sintering in an inert gas atmosphere to obtain a cemented carbide pre-sintered body; (3) The cemented carbide pre-sintered body is placed in a special reaction furnace for pressure sintering, vacuum sintered, and cooled to form a cemented carbide for cutting tools.

8. The method for preparing a cemented carbide for cutting tools according to claim 7, characterized in that: The inert gas is argon; the vacuum pressure is maintained at 30-45 MPa.

9. The method for preparing a cemented carbide for cutting tools according to claim 7, wherein the spark plasma sintering method maintains a current of 500-2000A and a voltage of 20-50V.

10. According to the method for preparing a cemented carbide for cutting tools as described in claim 7, in the spark plasma sintering, the temperature is first raised to 800-810°C, and sintered at this temperature for 1-2 minutes, and then the temperature is further raised to 1200-1300°C, and sintered at this temperature for 3-6 minutes; in the pressure sintering, the temperature is 1200-1350°C, and the sintering time is 1-2 hours.

Citation Information

Patent Citations

  • Hard alloy and preparation method thereof

    CN105714170A

  • Novel tungsten carbide composite material and preparation method thereof

    CN106747449A

  • Nano WC-Co hard alloy and preparation method thereof

    CN115044795A

  • Super-strong super-hard high-fracture-toughness hard alloy and preparation method thereof

    CN115305403A

  • ZrO2 toughened WC-TiC0.4 composite material and preparation method thereof

    CN116987942A