High-temperature-resistant and ultrahigh-strength plasticity AlCoCrFeNi high-entropy alloy material and preparation method thereof

By regulating the constituent elements and process treatment of AlCoCrFeNi high-entropy alloy, the problems of insufficient strength of nickel-based high-temperature alloy and the brittleness of refractory high-entropy alloy are solved, and the comprehensive improvement of high yield strength, compressive strength and plasticity is achieved, which significantly improves the material's High temperature resistance.

CN119020657APending Publication Date: 2024-11-26XIAN RARE METAL MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411136901.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing nickel-based high-temperature alloys are insufficient in aerospace applications. Refractory high-entropy alloys have limited their application range due to their brittleness, poor low-temperature ductility, poor high-temperature oxidation resistance and high density. They require a high-temperature resistant and ultra-high-strength plastic AlCoCrFeNi high Entropy alloy material.

Method used

By regulating the composition elements and atomic ratio of high-entropy alloy materials, the lattice distortion effect and nanophase precipitation effect are strengthened, and the solid solution strengthening, precipitation strengthening and co-element strengthening are added, combined with specific processes such as vacuum Smelting and surface grinding to remove impurities to improve the purity and stability of the alloy.

Benefits of technology

The strength and toughness and high temperature resistance of high entropy alloy materials are significantly improved, and the comprehensive improvement of high yield strength, compressive strength and plasticity is achieved, ensuring the excellent performance of the material at room temperature and high temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020657A_ABST
    Figure CN119020657A_ABST
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant and ultrahigh-strength plasticity AlCoCrFeNi high-entropy alloy material and a preparation method thereof.The atomic ratio of all the component elements of the material is AlaCobCrcFedNie, a is larger than or equal to 16 and smaller than or equal to 48, b is larger than or equal to 13 and smaller than or equal to 21, c is larger than or equal to 13 and smaller than or equal to 21, d is larger than or equal to 13 and smaller than or equal to 21, e is larger than or equal to 13 and smaller than or equal to 21, and a + b + c + d + e = 100; the preparation method comprises the following steps: 1, removing surface impurities from raw materials, cleaning, proportioning and weighing; 2, smelting; and 3, surface grinding and polishing. The composition elements and the atomic ratio of the high-entropy alloy material are regulated and controlled, the lattice distortion effect and the nanophase precipitation effect of the alloy are enhanced, the solid solution strengthening, precipitation strengthening and coherent strengthening effects of multi-principal component components are improved, and the obdurability and the high-temperature resistance of the material are enhanced; according to the preparation process, loss of low-melting-point raw materials is avoided, the influence of impurity elements is reduced, and the high-temperature resistance and obdurability of the material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material processing, and specifically relates to a high-temperature resistant, ultra-high-strength and plastic AlCoCrFeNi high-entropy alloy material and a preparation method thereof. Background Art

[0002] The development and application of structural materials with excellent abnormal temperature and high temperature performance is one of the important factors in promoting the development of science and technology. The aerospace industry needs new metal alloys for high temperature load-bearing structures and thermal protection systems. Currently, the popular structural material for aerospace is nickel-based high-temperature alloy, but the lack of strength has become a challenge for its further application.

[0003] As a new type of alloy, high entropy alloys have been developed for functional and structural applications and have shown a good combination of strength, ductility and high temperature resistance, which is superior to existing nickel-based high temperature alloys or refractory alloys. So far, refractory high entropy alloys are considered to be alloys with great potential for scientific and technological development due to their high melting points and excellent high temperature properties. For example, adding high temperature resistant molybdenum (Mo) and niobium (Nb) as alloying elements improves the strength and hardness of the alloy, but it is easy to form a brittle intermetallic compound phase. Its poor low temperature ductility, poor high temperature oxidation resistance and high density limit the application range of such refractory high entropy alloys.

[0004] Therefore, there is a need for a high-temperature resistant, ultra-high-strength and plastic AlCoCrFeNi high-entropy alloy material and a preparation method thereof. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a high temperature resistant, ultra-high strength and plastic AlCoCrFeNi high entropy alloy material in view of the deficiencies of the above-mentioned prior art. The method effectively strengthens the lattice distortion effect and nanophase precipitation effect of the alloy by regulating the constituent elements and atomic ratio of the high entropy alloy material, improves the solid solution strengthening, precipitation strengthening and coherent strengthening effects of the multi-principal component, enhances the toughness and high temperature resistance of the high entropy alloy material, and solves the problem that the high entropy alloy material is easy to form a brittle intermetallic compound phase and the strong plasticity and high temperature resistance are limited.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a high temperature resistant, ultra-high strength and plastic AlCoCrFeNi high entropy alloy material, characterized in that the high entropy alloy material has an atomic ratio of Al a Co b Cr c Fe d Ni e, wherein 16≤a≤48, 13≤b≤21, 13≤c≤21, 13≤d≤21, 13≤e≤21, and a+b+c+d+e=100; the high entropy alloy material has a yield strength of not less than 1400MPa, a compressive strength of not less than 3000MPa, and a plasticity of not less than 40% at room temperature, and a yield strength of not less than 400MPa, a compressive strength of not less than 600MPa, and a plasticity of not less than 50% at 800°C.

[0007] The high entropy alloy material of the present invention is beneficial to improving the ductility of the high entropy alloy by adding Co, Fe and Ni elements; and the addition of the brittle Cr element not only improves the high temperature resistance of the high entropy alloy, but also increases the strength of the high entropy alloy; at the same time, the addition of the Al element, which has a large difference in atomic radius from the three elements of Co, Fe and Ni, not only enhances the lattice distortion effect of the high entropy alloy and increases the solid solution strengthening effect of the high entropy alloy, but also forms an ordered B2 phase with the Ni element, thereby forming coherent strengthening of the BCC and B2 phases, and promotes the precipitation of the chromium-rich phase, further improving the strength and toughness of the high entropy alloy, so that the high entropy alloy material has excellent strong plasticity and high temperature resistance.

[0008] The above-mentioned high temperature resistant, ultra-high strength and plastic AlCoCrFeNi high entropy alloy material is characterized in that 18≤a≤45, 15≤b≤20, 15≤c≤20, 15≤d≤20, 15≤e≤20, and a+b+c+d+e=100.

[0009] The above-mentioned high temperature resistant, ultra-high strength and plastic AlCoCrFeNi high entropy alloy material is characterized in that a=40, b=15, c=15, d=15, and e=15. The plastic Co, Fe, and Ni elements added to the AlCoCrFeNi high entropy alloy material with this atomic ratio ensure the good plasticity of the high entropy alloy, the hard Cr element significantly enhances the strength of the high entropy alloy, and the solid solution strengthening, coherent strengthening, and precipitation strengthening brought about by the introduction of the Al element both enhance the strength of the high entropy alloy and improve the ductility of the high entropy alloy, so that the AlCoCrFeNi high entropy alloy material exhibits the best comprehensive performance.

[0010] In addition, the present invention also discloses a method for preparing the above-mentioned high temperature resistant, ultra-high strength and plastic AlCoCrFeNi high entropy alloy material, characterized in that the method comprises the following steps:

[0011] Step 1: Remove surface impurities from the raw materials Al, Co, Cr, Fe and Ni single metals, wash them in acetone, and then weigh them according to the designed alloy composition ratio;

[0012] Step 2: placing the raw materials weighed in step 1 into a vacuum melting furnace for melting to obtain a high entropy alloy ingot;

[0013] Step 3: Grind and polish the surface of the high entropy alloy ingot obtained in step 2 to obtain a high temperature resistant, ultra-high strength and plastic AlCoCrFeNi high entropy alloy material.

[0014] The present invention first removes carbon and oxygen impurities from the surface of metal raw materials Al, Co, Cr, Fe and Ni, and then puts them into a vacuum melting furnace for melting, and then polishes the surface to obtain a high-temperature resistant, ultra-high-strength and plastic AlCoCrFeNi high-entropy alloy. In the preparation process, the purity of the high-entropy alloy is ensured by first removing impurities such as carbon and oxides on the surface of the metal raw materials; at the same time, the placement of the metal raw materials in a specific order avoids the loss of elements, ensures the stability of the composition and structure, and further ensures that the AlCoCrFeNi high-entropy alloy has excellent strength, plasticity and high-temperature resistance.

[0015] The above method is characterized in that the mass purity of the Al, Co, Cr, Fe and Ni single metals in step 1 is greater than 99.95%, and the Al, Co, Cr, Fe and Ni single metals are all in granular or block form; the removal of impurities on the surface of the raw material is carried out by grinding with a grinding wheel machine. The present invention reduces the influence of carbon and oxides on the microstructure and mechanical properties of the high entropy alloy by controlling the raw material purification process, ensures the purity of the high entropy alloy, and is beneficial to the stability of the microstructure and mechanical properties of the high entropy alloy.

[0016] The above method is characterized in that the weighed raw materials in step 2 are placed in the following order: firstly, Al single metal is placed at the bottom of the crucible in the vacuum melting furnace, and then, Co, Cr, Fe, and Ni single metals are evenly mixed and placed on top of Al single metal. Compared with Co, Cr, Fe, and Nr elements, Al element has a lower melting point. In the present invention, Al raw material is first placed at the bottom of the crucible, and other raw materials are placed on top of Al raw material, thereby avoiding the loss of Al raw material and causing deviation of high entropy alloy composition during arc melting, thereby ensuring the stability of high entropy alloy composition, organization, and mechanical properties.

[0017] The above method is characterized in that before smelting in step 2, the smelting furnace is vacuumed to 1×10 -3 Pa, then fill with argon to 370Pa~420Pa, repeatedly evacuate and fill with argon 2~5 times, and perform gas washing operation on the melting furnace. Purifying and washing the melting furnace multiple times can remove the impurity gas in the melting furnace to the greatest extent, reduce the influence of gas impurities on the alloy, and ensure the stability of the microstructure and performance of the high entropy alloy.

[0018] Compared with the prior art, the present invention has the following advantages:

[0019] 1. The present invention effectively strengthens the lattice distortion effect of the alloy and the precipitation effect of the nanophase including the chromium-rich phase and the iron-chromium-rich phase by regulating the constituent elements and atomic ratio of the high entropy alloy material, adjusts the microstructure of the high entropy alloy, improves the solid solution strengthening, precipitation strengthening and coherent strengthening effects of the multi-principal component, and enhances the toughness and high temperature resistance of the high entropy alloy material.

[0020] 2. In the preparation process of the present invention, the placement and melting order of the metal raw materials are controlled according to the characteristics of the melting points of different metal raw materials, thereby avoiding the loss of low-melting-point raw materials, ensuring the stability of the high-entropy alloy composition and organizational structure, and improving the high-temperature resistance and toughness of the high-entropy alloy material.

[0021] 3. In the preparation process of the present invention, the smelting furnace is subjected to gas washing treatment, which effectively removes the impurity gas in the smelting furnace, reduces the influence of the impurity elements on the high entropy alloy, ensures the purity of the high entropy alloy, stabilizes the organizational structure of the high entropy alloy, and improves the high temperature resistance and strong plasticity of the high entropy alloy material.

[0022] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Room temperature and high temperature compressive stress-strain curves of the AlCoCrFeNi high entropy alloy material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0024] Example 1

[0025] The AlCoCrFeNi high entropy alloy material of this embodiment is composed of Al 40 Co 15 Cr 15 Fe 15 Ni 15 .

[0026] The preparation method of the AlCoCrFeNi high entropy alloy material of this embodiment comprises the following steps:

[0027] Step 1: Grind Al, Co, Cr, Fe and Ni granular single substances with a mass purity greater than 99.95% with a grinder to remove surface impurities, wash them in acetone, and then weigh them according to the designed alloy composition ratio;

[0028] Step 2: Place the Al granular element weighed in step 1 at the bottom of the crucible in the vacuum melting furnace, then evenly mix the Co, Cr, Fe, and Ni granular elements and place them on top of the Al granular element to cover it, and evacuate the vacuum melting furnace to 1×10 -3Pa, then fill with argon to 370Pa, repeatedly evacuate and fill with argon for 3 times, perform gas washing operation on the melting furnace, then open the melting arc to perform multiple reversal melting of Al, Co, Cr, Fe, and Ni granular single substances to obtain high entropy alloy ingots;

[0029] Step 3: Grind and polish the surface of the high entropy alloy ingot obtained in step 2 to obtain an AlCoCrFeNi high entropy alloy material.

[0030] After testing, such as Figure 1 As shown in Figures (a) and (b), the AlCoCrFeNi high entropy alloy material prepared in this embodiment has a yield strength of 1454 MPa, a compressive strength of 3628 MPa, and a plasticity of 47.7% at room temperature, a yield strength of 448 MPa, a compressive strength of 660 MPa, and a plasticity of 60.1% at 800°C, indicating that the AlCoCrFeNi high entropy alloy material has excellent high temperature resistance and ultra-high strength and plasticity.

[0031] Example 2

[0032] The AlCoCrFeNi high entropy alloy material of this embodiment is composed of Al 48 Co 13 Cr 13 Fe 13 Ni 13 .

[0033] The preparation method of the AlCoCrFeNi high entropy alloy material of this embodiment comprises the following steps:

[0034] Step 1: Use a grinding machine to grind Al, Co, Cr, Fe and Ni bulk single substances with a mass purity greater than 99.95% to remove surface impurities, then wash them in acetone, and then weigh them according to the designed alloy composition ratio;

[0035] Step 2: Place the Al bulk element weighed in step 1 at the bottom of the crucible in the vacuum melting furnace, then mix the Co, Cr, Fe, and Ni bulk elements evenly and place them on top of the Al bulk element to cover it, and evacuate the vacuum melting furnace to 1×10 -3 Pa, then fill with argon to 420Pa, repeatedly evacuate and fill with argon 4 times, perform gas washing operation on the melting furnace, then open the melting arc to perform multiple flip melting of Al, Co, Cr, Fe, and Ni bulk single substances to obtain high entropy alloy ingots;

[0036] Step 3: Grind and polish the surface of the high entropy alloy ingot obtained in step 2 to obtain an AlCoCrFeNi high entropy alloy material.

[0037] After testing, the AlCoCrFeNi high entropy alloy material prepared in this embodiment has a yield strength of 1483 MPa, a compressive strength of 3421 MPa, and a plasticity of 41% at room temperature, and a yield strength of 467 MPa, a compressive strength of 689 MPa, and a plasticity of 57% at 800°C, indicating that the AlCoCrFeNi high entropy alloy material has excellent high temperature resistance and ultra-high strength and plasticity.

[0038] Example 3

[0039] The AlCoCrFeNi high entropy alloy material of this embodiment is composed of Al 16 Co 21 Cr 21 Fe 21 Ni 21 .

[0040] The preparation method of the AlCoCrFeNi high entropy alloy material of this embodiment comprises the following steps:

[0041] Step 1: Use a grinding machine to grind Al, Co, Cr, Fe and Ni bulk single substances with a mass purity greater than 99.95% to remove surface impurities, then wash them in acetone, and then weigh them according to the designed alloy composition ratio;

[0042] Step 2: Place the Al bulk element weighed in step 1 at the bottom of the crucible in the vacuum melting furnace, then mix the Co, Cr, Fe, and Ni bulk elements evenly and place them on top of the Al bulk element to cover it, and evacuate the vacuum melting furnace to 1×10 -3 Pa, then fill with argon to 410Pa, repeatedly evacuate and fill with argon twice, perform gas washing operation on the melting furnace, then open the melting arc to perform multiple flip melting of Al, Co, Cr, Fe, and Ni bulk single substances to obtain high entropy alloy ingots;

[0043] Step 3: Grind and polish the surface of the high entropy alloy ingot obtained in step 2 to obtain an AlCoCrFeNi high entropy alloy material.

[0044] After testing, the AlCoCrFeNi high entropy alloy material prepared in this embodiment has a yield strength of 1411 MPa, a compressive strength of 3024 MPa, and a plasticity of 45% at room temperature, and a yield strength of 405 MPa, a compressive strength of 623 MPa, and a plasticity of 62% at 800°C, indicating that the AlCoCrFeNi high entropy alloy material has excellent high temperature resistance and ultra-high strength and plasticity.

[0045] Example 4

[0046] The AlCoCrFeNi high entropy alloy material of this embodiment is composed of Al45 Co 14 Cr 14 Fe 14 Ni 13 .

[0047] The preparation method of the AlCoCrFeNi high entropy alloy material of this embodiment comprises the following steps:

[0048] Step 1: Grind Al, Co, Cr, Fe and Ni granular single substances with a mass purity greater than 99.95% with a grinder to remove surface impurities, wash them in acetone, and then weigh them according to the designed alloy composition ratio;

[0049] Step 2: Place the Al granular element weighed in step 1 at the bottom of the crucible in the vacuum melting furnace, then mix the Co, Cr, Fe, and Ni granular elements evenly and place them on top of the Al granular element to cover it, and then evacuate the vacuum melting furnace to 1×10 -3 Pa, then fill with argon to 400Pa, repeatedly evacuate and fill with argon 5 times, perform gas washing operation on the melting furnace, then open the melting arc to perform multiple flip melting of Al, Co, Cr, Fe, Ni granular single substances to obtain high entropy alloy ingots;

[0050] Step 3: Grind and polish the surface of the high entropy alloy ingot obtained in step 2 to obtain an AlCoCrFeNi high entropy alloy material.

[0051] After testing, the AlCoCrFeNi high entropy alloy material prepared in this embodiment has a yield strength of 1440 MPa, a compressive strength of 3468 MPa, and a plasticity of 43.5% at room temperature; a yield strength of 430 MPa, a compressive strength of 643 MPa, and a plasticity of 67% at 800°C, indicating that the AlCoCrFeNi high entropy alloy material has excellent high temperature resistance and ultra-high strength and plasticity.

[0052] Example 5

[0053] The AlCoCrFeNi high entropy alloy material of this embodiment is composed of Al 20 Co 20 Cr 20 Fe 20 Ni 20 .

[0054] The preparation method of the AlCoCrFeNi high entropy alloy material of this embodiment comprises the following steps:

[0055] Step 1: Use a grinding machine to grind Al, Co, Cr, Fe and Ni bulk single substances with a mass purity greater than 99.95% to remove surface impurities, then wash them in acetone, and then weigh them according to the designed alloy composition ratio;

[0056] Step 2: Place the Al bulk element weighed in step 1 at the bottom of the crucible in the vacuum melting furnace, then mix the Co, Cr, Fe, and Ni bulk elements evenly and place them on top of the Al bulk element to cover it, and evacuate the vacuum melting furnace to 1×10 -3 Pa, then fill with argon to 390Pa, repeatedly evacuate and fill with argon for 3 times, perform gas washing operation on the melting furnace, then open the melting arc to perform multiple flip melting of Al, Co, Cr, Fe, and Ni bulk single substances to obtain high entropy alloy ingots;

[0057] Step 3: Grind and polish the surface of the high entropy alloy ingot obtained in step 2 to obtain an AlCoCrFeNi high entropy alloy material.

[0058] After testing, the AlCoCrFeNi high entropy alloy material prepared in this embodiment has a yield strength of 1426 MPa, a compressive strength of 3354 MPa, and a plasticity of 48.3% at room temperature, and a yield strength of 428 MPa, a compressive strength of 654 MPa, and a plasticity of 68% at 800°C, indicating that the AlCoCrFeNi high entropy alloy material has excellent high temperature resistance and ultra-high strength and plasticity.

[0059] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A high temperature resistant, ultra-high strength and plastic AlCoCrFeNi high entropy alloy material, characterized in that: The high entropy alloy material is composed of Al a Co b Cr c Fe d Ni e , wherein 16≤a≤48, 13≤b≤21, 13≤c≤21, 13≤d≤21, 13≤e≤21, and a+b+c+d+e=100; the high entropy alloy material has a yield strength of not less than 1400MPa, a compressive strength of not less than 3000MPa, and a plasticity of not less than 40% at room temperature, and a yield strength of not less than 400MPa, a compressive strength of not less than 600MPa, and a plasticity of not less than 50% at 800°C.

2. The high temperature resistant, ultra-high strength and plastic AlCoCrFeNi high entropy alloy material according to claim 1, characterized in that: 18≤a≤45, 15≤b≤20, 15≤c≤20, 15≤d≤20, 15≤e≤20, and a+b+c+d+e=100.

3. A high temperature resistant, ultra-high strength and plastic AlCoCrFeNi high entropy alloy material according to claim 2, characterized in that: a=40, b=15, c=15, d=15, e=15.

4. A method for preparing a high temperature resistant, ultra-high strength and plastic AlCoCrFeNi high entropy alloy material as claimed in any one of claims 1 to 3, characterized in that: The method comprises the following steps: Step 1: Remove surface impurities from the raw materials Al, Co, Cr, Fe and Ni single metals, wash them in acetone, and then weigh them according to the designed alloy composition ratio; Step 2: placing the raw materials weighed in step 1 into a vacuum melting furnace for melting to obtain a high entropy alloy ingot; Step 3: Grind and polish the surface of the high entropy alloy ingot obtained in step 2 to obtain a high temperature resistant, ultra-high strength and plastic AlCoCrFeNi high entropy alloy material.

5. The method according to claim 4, characterized in that The mass purity of the Al, Co, Cr, Fe and Ni single metals in step 1 is greater than 99.95%, and the Al, Co, Cr, Fe and Ni single metals are all in granular or block form; the removal of impurities on the surface of the raw material is carried out by grinding with a grinding wheel machine.

6. The method according to claim 4, characterized in that The weighed raw materials in step 2 are placed in the following order: firstly, Al single metal is placed at the bottom of the crucible in the vacuum melting furnace, and then, Co, Cr, Fe, and Ni single metals are evenly mixed and placed on top of the Al single metal.

7. The method according to claim 4, characterized in that Before smelting in step 2, the smelting furnace is vacuumed to 1×10 -3 Pa, and then fill with argon to 370Pa~420Pa, repeatedly evacuate and fill with argon 2~5 times, and perform gas washing operation on the smelting furnace.