Method for preparing iron-based resistance alloy plate based on rolling annealing process, prepared iron-based resistance alloy plate and application

By using the rolling and annealing process in precision resistive alloys, the annealing temperature and time are regulated and the face-centered cubic phase is generated, and the problem of insufficient resistivity and mechanical properties in the prior art is solved, and the combination of high resistivity and excellent mechanical properties is achieved. .

CN119020661AInactive Publication Date: 2024-11-26SHAANXI SCI TECH UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410819774.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The resistivity of existing precision resistance alloys does not meet the scope of precision resistance alloys after cold rolling and heat treatment, and the resistance temperature coefficient is high and the mechanical properties are poor.

Method used

Using a method based on the rolling and annealing process, the Fe, Cr, Co, W metal materials are melted and homogenized, and then cold rolled, annealing treatment is performed at 1223-1323K under a protective atmosphere to regulate the annealing temperature and time. , generate face-centered cubic phase, change grain size and defect density, and improve the resistivity and mechanical properties of the alloy.

Benefits of technology

The high resistivity is maintained and the mechanical properties of the alloy are significantly improved, ensuring the stability and applicability of alloy sheets in practical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020661A_ABST
    Figure CN119020661A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing an iron-based resistance alloy plate based on a rolling annealing process, the prepared iron-based resistance alloy plate and application, and belongs to the technical field of alloy materials. The method comprises the following steps: smelting and homogenizing Fe, Cr, Co and W metal materials to obtain an alloy; the alloy is composed of the following components in percentage by mass: 50-60 wt% of Fe, 14-20 wt% of Cr, 20-23 wt% of Co and 4-7 wt% of W, totaling 100%. The alloy is subjected to cold rolling treatment, the cold rolling pressing amount is 10-90%, and a cold-rolled alloy plate is obtained; and after the cold-rolled alloy plate is sliced, annealing treatment is conducted under the protective atmosphere and the condition of 1223 K to 1323 K, the grain size and defect density of the alloy are changed through the annealing treatment, a face-centered cubic phase is generated, and the iron-based resistance alloy plate is obtained. The iron-based resistance alloy plate prepared by the preparation method disclosed by the invention not only keeps relatively high resistivity, but also has excellent mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of alloy materials, and more specifically to a method for preparing an iron-based resistance alloy plate based on a rolling annealing process, and the prepared iron-based resistance alloy plate and its application. Background Art

[0002] Precision resistance alloy is a kind of resistance alloy with high resistivity (≥100μΩ·cm) and low resistance temperature coefficient. It is the basic material for making resistance instruments, measuring instruments and resistance elements of other industrial devices. It has been widely used in defense industry, mobile communications, automotive electronics and other industries.

[0003] At present, the precision resistor alloys used in various precision instruments need to be foils or thin plates with the advantages of easy adhesion, miniaturization and large area, such as strain gauges installed on the elastic elements of strain-type force sensors. Not only are the electrical properties of the alloys required, but the alloys also need to have a certain strength to bear external forces. Therefore, it is necessary to roll the alloy to obtain the required foil or thin plate to meet the actual application needs. Studies have shown that the alloy not only has a large number of defects after cold rolling, but also has severe work hardening.

[0004] The researchers studied the Cu-7Mn-0.5Ag-0.2Ce-0.2Zr resistance alloy, which was subjected to 90% cold rolling deformation and annealed at 623K for 1h to obtain an alloy with a resistivity of 24.1μΩ·cm and a resistance temperature coefficient of 60ppm / ℃. It can be found that the resistivity of the alloy after cold rolling and heat treatment does not meet the category of precision resistance alloys, and the resistance temperature coefficient is high and the mechanical properties are poor. Summary of the invention

[0005] In view of the above problems, the present invention provides a method for preparing an iron-based resistance alloy plate based on a rolling annealing process. The iron-based resistance alloy plate prepared by the present invention not only maintains a relatively high resistivity, but also has excellent mechanical properties.

[0006] In a first aspect, the present invention provides a method for preparing an iron-based resistance alloy plate based on a rolling annealing process, comprising the following steps:

[0007] An alloy obtained by smelting and homogenizing Fe, Cr, Co and W metal materials; the alloy consists of the following components in mass percentage: Fe 50-60wt%, Cr 14-20wt%, Co 20-23wt%, W 4-7wt%, totaling 100%;

[0008] The alloy is cold rolled with a cold rolling reduction of 10-90% to obtain a cold rolled alloy sheet;

[0009] The cold-rolled alloy sheet is sliced ​​and then annealed under a protective atmosphere at 1223-1323 K. The grain size and defect density of the alloy are changed by the annealing treatment, and a face-centered cubic phase is generated to obtain an iron-based resistance alloy sheet.

[0010] For example, the annealing temperature is 1223K, 1233K, 1243K, 1253K, 1263K, 1273K, 1283K, 1293K, 1303K, 1313K, 1323K, etc.

[0011] However, it is not limited to the listed values. Other values ​​not listed within the above numerical range are also applicable and will not be detailed here.

[0012] The alloy is composed of the following components in percentage by mass: Fe 50-60wt%, Cr 14-20wt%, Co 20-23wt%, W 4-7wt%, totaling 100%;

[0013] For example, the mass percentage of Fe in the iron-based resistance alloy is 50wt%, 51wt%, 52wt%, 53wt%, 54wt%, 55wt%, 56wt%, 57wt%, 58wt%, 59wt%, 60wt%, etc.;

[0014] The mass percentage of Cr in the iron-based resistance alloy is 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, etc.;

[0015] The mass percentage of Co in the iron-based resistance alloy is 20wt%, 21wt%, 22wt%, 23wt%, etc.;

[0016] The mass percentage of W in the iron-based resistance alloy is 4wt%, 5wt%, 6wt%, 7wt%, etc.;

[0017] However, it is not limited to the listed values. Other values ​​not listed within the above numerical range are also applicable and will not be detailed here.

[0018] As a preferred technical solution of the present invention, the annealing temperature is 1223K.

[0019] As a preferred technical solution of the present invention, the annealing time is 1-1.5h. It is understandable that the annealing temperature and the length of time will affect the grain size of the alloy, and directly affect the electrical and mechanical properties of the alloy. Within the above parameter range, generally speaking, if the annealing temperature is too high, secondary recrystallization will occur inside the alloy, the grains will grow abnormally, and the performance will decrease; if the annealing temperature is too low, the residual stress generated during the cold deformation process cannot be fully released, the crystal defect density is high, and it is difficult to keep the character of the alloy stable. If the annealing time is too short, the grains of the alloy will not have time to grow, which will cause unstable performance; if the annealing time is too long, the grains will grow abnormally, and the electrical and mechanical properties of the alloy will decrease instead.

[0020] For example, the annealing time is 1h, 70min, 80min, 1.5h, etc.

[0021] However, it is not limited to the listed values. Other values ​​not listed within the above numerical range are also applicable and will not be detailed here.

[0022] As a preferred technical solution of the present invention, the annealing time is 1 hour.

[0023] As a preferred technical solution of the present invention, the number of cold rolling is 1-5 times, and the single pressing amount is 10-20%. The change of the number of cold rolling and the single pressing amount will affect the thickness of the alloy plate, thereby affecting the electrical and mechanical properties of the alloy plate.

[0024] For example, the number of cold rolling times is 1, 2, 3, 4, 5, etc.;

[0025] The single pressure amount is 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, etc.

[0026] However, it is not limited to the listed values. Other values ​​not listed within the above numerical range are also applicable and will not be detailed here.

[0027] As a preferred technical solution of the present invention, the thickness of the alloy sheet after cold rolling is 0.5-4.5 mm. Within this parameter range, if the thickness is too large, it will bring many inconveniences in practical application.

[0028] For example, the thickness of the alloy sheet after cold rolling can be 0.5 mm, 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm, 4.5 mm, etc.

[0029] However, it is not limited to the listed values. Other values ​​not listed within the above numerical range are also applicable and will not be detailed here.

[0030] As a preferred technical solution of the present invention, the alloy consists of the following components in mass percentage: Fe 56.5wt%, Cr 14wt%, Co 23wt%, and W 6.5wt%.

[0031] In a second aspect, the present invention provides an iron-based resistance alloy plate material prepared according to the preparation method described in the first aspect.

[0032] In a third aspect, the present invention provides an application of the iron-based resistance alloy plate material according to the second aspect in a patch-type strain resistance sensor.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] The present invention uses Fe, Cr, Co and W as raw materials, performs cold rolling and annealing after smelting and homogenization. In the annealing process, the annealing temperature is regulated to be 1223-1323K. Within this temperature range, the grains of the alloy grow to some extent, thereby maintaining the resistivity of the alloy plate to be greater than 100μΩ·cm. In addition, the annealing treatment is used to regulate the appearance of a face-centered cubic phase in the alloy plate, and the plasticity of the alloy plate is improved by the face-centered cubic phase, thereby ensuring that the alloy plate has excellent mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 is the XRD spectrum of the alloy of Example 1;

[0036] Figure 2 This is the electron backscattering (EBSD) analysis diagram of the alloy in Example 1;

[0037] Figure 3 is the tensile curve of Example 1;

[0038] Figure 4 is the XRD spectrum of Example 2;

[0039] Figure 5 It is the tensile curve diagram of Example 2;

[0040] Figure 6 is the XRD spectrum of Example 3;

[0041] Figure 7 This is the electron backscatter (EBSD) analysis diagram of Example 3;

[0042] Figure 8 is the tensile curve diagram of Example 3;

[0043] Fig. 9 is the XRD spectrum of Example 4;

[0044] Fig.10 This is the electron backscattering (EBSD) analysis diagram of Example 4;

[0045] Fig.11 is the tensile curve diagram of Example 4;

[0046] Fig.12 is the XRD spectrum of the alloy of Comparative Example 1;

[0047] Fig.13 The scanning electron microscope morphology and X-ray energy spectrum (EDS) surface scan of the alloy in comparative example 1;

[0048] Fig.14 This is the tensile curve of the alloy in comparative example 1. DETAILED DESCRIPTION

[0049] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0050] In a complete crystal, electrons basically move in a uniform electric field and no scattering occurs. When the alloy is deformed by cold working, a large number of crystal defects will be generated, the lattice period will be destroyed, and the electric field will change sharply, which will produce a strong scattering effect on the electrons, resulting in an increase in the resistivity of the alloy, but the plasticity of the alloy will be significantly reduced, reducing the comprehensive mechanical properties of the alloy. After the cold-worked alloy is annealed, the crystal defects in the alloy gradually decrease, weakening the electron scattering, the resistivity may decrease, and the plasticity of the alloy will be improved. The strength of the annealed alloy is reduced, which can be attributed to three reasons, namely the reduction of dislocation density, the weakening of texture strength and the release of stress. First, the high-density dislocations will be transformed into subgrain boundary structures during the annealing process, transformed into high-angle grain boundaries and developed into recrystallized grains. The reduction in dislocation density further causes the strength of the alloy to decrease. Secondly, the strong texture strength makes the material have a higher strength in the rolling direction. The sharp decrease in texture strength after annealing will also cause the strength of the alloy to decrease. Finally, a large number of equiaxed grains are formed through recrystallization, which releases a large amount of stress and leads to a decrease in mechanical properties.

[0051] Based on this, the present invention provides a method for preparing an iron-based resistance alloy plate based on a rolling annealing process, wherein the four materials of Fe, Cr, Co, and W are subjected to smelting and homogenization treatment, and then cold-rolled to obtain an alloy plate of suitable thickness through cold-rolling treatment, and then annealed, and the annealing temperature is adjusted to 1223-1323K. Within this temperature range, the grain size and defect density are controlled to maintain the resistivity of the alloy plate greater than 100μΩ·cm. In essence, the degree of electron scattering is aggravated or weakened by increasing or reducing the crystal defects in the alloy, and the resistivity of the alloy is further adjusted. In addition, the face-centered cubic phase appears in the alloy plate through annealing treatment, and the plasticity of the alloy plate is improved through the face-centered cubic phase, thereby ensuring that the alloy plate has excellent mechanical properties.

[0052] Example 1

[0053] Step 1: According to the chemical formula Fe 56.5 Cr 14 Co 23 W 6.5 (mass percentage) for batching, the raw materials used are blocks corresponding to the purity of each element greater than 99.90%;

[0054] Step 2: Use a vacuum induction magnetic levitation melting furnace (AM800-3, Hefei Kejing Material Technology Co., Ltd.) to melt in an argon protective atmosphere until the vacuum degree reaches 10 -3 After Pa, argon gas was filled until the pressure returned to normal slightly, the melting temperature was 1773K, the melting was repeated 4 times, and the rectangular alloy ingot was cast at 1873K;

[0055] Step 3: After obtaining the smelted ingot, the alloy is homogenized in a box furnace (KSL-1800x-A1-W) in an argon protective atmosphere at a homogenization temperature of 1473K for 2 hours, followed by furnace cooling;

[0056] Step 4: cold rolling the alloy using a four-roller rolling mill, with a single rolling reduction of 20% and a total rolling reduction of 60%, to obtain an alloy sheet with a thickness of 2 mm;

[0057] Step 5: Slice the cold-rolled alloy sheet to obtain samples with a size of 12 mm × 10 mm × 2 mm, and anneal them in a vacuum tube furnace (GSL_1600X) filled with argon at a temperature of 1223 K for 1 h to obtain annealed alloy sheets.

[0058] The XRD spectrum of the alloy obtained in Example 1 is as follows: Figure 1 As shown, from Figure 1The XRD spectrum of the alloy shows that there are body-centered cubic (BCC) and a small amount of face-centered cubic (FCC) structures. The increase of annealing temperature generates FCC phase, which improves the plasticity of the alloy to a certain extent. Figure 2 This is the EBSD test image. It can be seen that the content percentage of BCC phase in the alloy is 98.6% and the content percentage of FCC phase is 2.4%. Figure 2 (b) is the inverse pole figure of the alloy. It is found that the grains of different colors are evenly distributed, indicating that the degree of preferred orientation of the alloy decreases after annealing, indicating that the proportion of any texture is not prominent. The average LAM is calculated to be 0.25° and the average dislocation density is 4.73×10 13 m -2 . Figure 3 is the engineering stress-strain tensile curve of the alloy, Figure 3 It can be seen that the yield strength of the alloy is 598MPa, the tensile strength is 1006MPa, and the uniform elongation is 9.4%. The resistivity of the alloy is 123.7μm·cm, and the temperature coefficient of resistance is 6.0×10 -4 ppm / ℃.

[0059] After 60% cold deformation, the resistivity of the alloy is 140.0μm·cm. After annealing at 1223K, the resistivity of the alloy is reduced to 123.7μm·cm. This is mainly because after annealing, the grain size of the alloy increases, the number of grain boundaries decreases, and the electron scattering caused by the grain boundaries is reduced. At the same time, the lattice integrity of the alloy is restored after annealing, the crystal defects are greatly reduced, and the electron scattering effect is weakened, resulting in a decrease in resistivity. Secondly, the dislocation density of the alloy after annealing decreases by nearly an order of magnitude compared with that before annealing. Therefore, the contribution of dislocation density to the resistivity of the alloy is also weakened.

[0060] As for the mechanical properties of the alloy sheet, the yield strength and uniform elongation are 598 MPa and 9.4% respectively. This is because the appearance of the FCC phase is conducive to the improvement of plasticity. The present invention changes the amount of the FCC phase in the alloy by regulating the annealing temperature, thereby improving the mechanical properties of the alloy sheet.

[0061] Example 2

[0062] Step 1: According to the chemical formula Fe 56.5 Cr 14 Co 23 W 6.5 (mass percentage) for batching, the raw materials used are blocks corresponding to the purity of each element greater than 99.8%;

[0063] Step 2: Use vacuum arc melting (AM800-3, Hefei Kejing Material Technology Co., Ltd.) to melt in an argon protective atmosphere until the vacuum degree reaches 10-3 After Pa, argon gas was filled until the pressure returned to normal slightly, the melting temperature was 1773K, the melting was repeated 4 times, and the rectangular alloy ingot was cast at 1873K;

[0064] Step 3: After obtaining the smelted ingot, the alloy is homogenized in a box furnace (KSL-1800x-A1-W) in an argon protective atmosphere at a homogenization temperature of 1473K for 2 hours, followed by furnace cooling;

[0065] Step 4: cold rolling the alloy using a four-roller rolling mill, with a single rolling reduction of 20% and a total rolling reduction of 80% to obtain an alloy sheet with a thickness of 1 mm;

[0066] Step 5: Slice the cold-rolled alloy sheet to obtain samples with a size of 12 mm × 10 mm × 2 mm, and anneal them in a vacuum tube furnace (GSL_1600X) filled with argon at a temperature of 1223 K for 1 h to obtain annealed alloy sheets.

[0067] The XRD spectrum of the alloy obtained in Example 2 is as follows Figure 4 As shown in Figure 2, it can be seen that there are body-centered cubic (BCC) and a small amount of face-centered cubic (FCC) structures in the alloy. Figure 5 is the engineering stress-strain tensile curve of the alloy, Figure 5 It can be seen that the yield strength of the alloy is 562MPa, the tensile strength is 1000MPa, and the uniform elongation is 8.2%. The FCC phase that appears after annealing is conducive to plasticity and the strength is not significantly reduced. The resistivity of the alloy is 120.7μm·cm, and the temperature coefficient of resistance is 6.2×10 -4 ppm / ℃.

[0068] Example 3

[0069] Step 1: According to the chemical formula Fe 56.5 Cr 14 Co 23 W 6.5 (mass percentage) for batching, the raw materials used are blocks corresponding to the purity of each element greater than 99.8%;

[0070] Step 2: Use vacuum arc melting (AM800-3, Hefei Kejing Material Technology Co., Ltd.) to melt in an argon protective atmosphere until the vacuum degree reaches 10 -3 After Pa, argon gas was filled until the pressure returned to normal slightly, the melting temperature was 1773K, the melting was repeated 4 times, and the rectangular alloy ingot was cast at 1873K;

[0071] Step 3: After obtaining the smelted ingot, the alloy is homogenized in a box furnace (KSL-1800x-A1-W) in an argon protective atmosphere at a homogenization temperature of 1473K for 2 hours, followed by furnace cooling;

[0072] Step 4: cold rolling the alloy using a four-roller rolling mill, with a single rolling reduction of 20% and a total rolling reduction of 90%, to obtain an alloy sheet with a thickness of 0.5 mm;

[0073] Step 5: Slice the cold-rolled alloy sheet to obtain samples with a size of 12 mm × 10 mm × 2 mm, and anneal them in a vacuum tube furnace (GSL_1600X) filled with argon at a temperature of 1223 K for 1 h to obtain annealed alloy sheets.

[0074] The XRD spectrum of the alloy obtained in Example 3 is as follows Figure 6 As shown. Figure 6 The XRD spectra of the alloys showed body-centered cubic (BCC) and face-centered cubic (FCC) structures. Figure 7 This is the EBSD test image. It can be seen that the BCC phase content in the alloy accounts for 98.8% and the FCC phase content accounts for 1.2%. Figure 7 (b) is the inverse pole figure of the alloy. It is found that the grains of different colors are evenly distributed, indicating that the degree of preferred orientation of the alloy decreases after annealing, indicating that the proportion of any texture is not prominent. The average LAM is calculated to be 0.24° and the average dislocation density is 4.83×10 13 m -2 . Figure 8 is the engineering stress-strain tensile curve of the alloy, Figure 8 It can be seen that the yield strength of the alloy is 670MPa, the tensile strength is 1017MPa, and the uniform elongation is 8.8%. The FCC phase that appears after annealing is conducive to plasticity and the strength is not significantly reduced, which may be due to the amount of FCC precipitated at this temperature. The resistivity of the alloy in the alloy reaches 146.3μm·cm, and the temperature coefficient of resistance is 6.3×10 -4 ppm / ℃.

[0075] Example 4

[0076] Step 1: According to the chemical formula Fe 56.5 Cr 14 Co 23 W 6.5 (mass percentage) for batching, the raw materials used are blocks corresponding to the purity of each element greater than 99.8%;

[0077] Step 2: Use vacuum arc melting (AM800-3, Hefei Kejing Material Technology Co., Ltd.) to melt in an argon protective atmosphere until the vacuum degree reaches 10 -3 After Pa, argon gas was filled until the pressure returned to normal slightly, the melting temperature was 1773K, the melting was repeated 4 times, and the rectangular alloy ingot was cast at 1873K;

[0078] Step 3: After obtaining the smelted ingot, the alloy is homogenized in a box furnace (KSL-1800x-A1-W) in an argon protective atmosphere at a homogenization temperature of 1473K for 2 hours, followed by furnace cooling;

[0079] Step 4: cold rolling the alloy using a four-roller rolling mill, with a single rolling reduction of 20% and a total rolling reduction of 60%, to obtain an alloy sheet with a thickness of 2 mm;

[0080] Step 5: Slice the cold-rolled alloy sheet to obtain samples with a size of 12 mm × 10 mm × 2 mm, and anneal them in a vacuum tube furnace (GSL_1600X) filled with argon at a temperature of 1323 K for 1 h to obtain annealed alloy sheets.

[0081] The XRD spectrum of the alloy obtained in Example 4 is as follows Fig. 9 As shown. Fig. 9 The XRD spectra of the alloys showed body-centered cubic (BCC) and face-centered cubic (FCC) structures. Fig.10 This is the EBSD test image. It can be observed that the BCC content in the alloy accounts for 94.6% and the FCC phase content accounts for 5.4%. Fig.10 (b) is the inverse pole figure of the alloy. It is found that the grains of different colors are evenly distributed, indicating that the degree of preferred orientation of the alloy decreases after annealing, indicating that the proportion of any texture is not prominent. The average LAM is calculated to be 0.20° and the average dislocation density is 3.52×10 13 m -2 . Fig.11 is the engineering stress-strain tensile curve of the alloy, Fig.11 It can be seen that the yield strength of the alloy is 401MPa, the tensile strength is 1008MPa, and the uniform elongation is 13.3%. The uniform elongation of the alloy at this annealing temperature is relatively high. This is because the higher the annealing temperature, the more FCC phases are precipitated, and the better the plasticity of the alloy. The resistivity of the alloy is 107.1μm·cm, and the temperature coefficient of resistance is 0.083ppm / ℃.

[0082] The increase in annealing temperature causes the grain size and dislocation density of the alloy to increase compared with Example 1, weakens electron scattering, and reduces the resistivity of the alloy.

[0083] Example 5

[0084] Step 1: According to the chemical formula Fe 58 Cr 15 Co 20 W7 (mass percentage) is used for batching, and the raw materials use blocks corresponding to the purity of each element greater than 99.8%;

[0085] Step 2: Use vacuum arc melting (AM800-3, Hefei Kejing Material Technology Co., Ltd.) to melt in an argon protective atmosphere until the vacuum degree reaches 10 -3 After Pa, argon gas was filled until the pressure returned to normal slightly, the melting temperature was 1773K, the melting was repeated 4 times, and the rectangular alloy ingot was cast at 1873K;

[0086] Step 3: After obtaining the smelted ingot, the alloy is homogenized in a box furnace (KSL-1800x-A1-W) in an argon protective atmosphere at a homogenization temperature of 1473K for 2 hours, followed by furnace cooling;

[0087] Step 4: cold rolling the alloy using a four-roller rolling mill, with a single rolling reduction of 10% and a total rolling reduction of 10%, to obtain an alloy sheet with a thickness of 4.5 mm;

[0088] Step 5: Slice the cold-rolled alloy sheet to obtain samples with a size of 12 mm × 10 mm × 2 mm, and anneal them in a vacuum tube furnace (GSL_1600X) filled with argon at a temperature of 1223 K for 1.5 h to obtain annealed alloy sheets.

[0089] Example 6

[0090] Step 1: According to the chemical formula Fe 60 Cr 14 Co 22 W4 (mass percentage) is used for batching, and the raw materials use blocks corresponding to the purity of each element greater than 99.8%;

[0091] Step 2: Use vacuum arc melting (AM800-3, Hefei Kejing Material Technology Co., Ltd.) to melt in an argon protective atmosphere until the vacuum degree reaches 10 -3 After Pa, argon gas was filled until the pressure returned to normal slightly, the melting temperature was 1773K, the melting was repeated 4 times, and the rectangular alloy ingot was cast at 1873K;

[0092] Step 3: After obtaining the smelted ingot, the alloy is homogenized in a box furnace (KSL-1800x-A1-W) in an argon protective atmosphere at a homogenization temperature of 1473K for 2 hours, followed by furnace cooling;

[0093] Step 4: cold rolling the alloy using a four-roller rolling mill, with a single rolling reduction of 15% and a total rolling reduction of 60%, to obtain an alloy sheet with a thickness of 3 mm;

[0094] Step 5: Slice the cold-rolled alloy sheet to obtain a sample with a size of 12 mm × 10 mm × 2 mm, and anneal it in a vacuum tube furnace (GSL_1600X) filled with argon at a temperature of 1323 K for 1.2 h to obtain an annealed alloy sheet.

[0095] Example 7

[0096] Step 1: According to the chemical formula Fe 50 Cr 20 Co 23 W7 (mass percentage) is used for batching, and the raw materials use blocks corresponding to the purity of each element greater than 99.8%;

[0097] Step 2: Use vacuum arc melting (AM800-3, Hefei Kejing Material Technology Co., Ltd.) to melt in an argon protective atmosphere until the vacuum degree reaches 10 -3 After Pa, argon gas was filled until the pressure returned to normal slightly, the melting temperature was 1773K, the melting was repeated 4 times, and the rectangular alloy ingot was cast at 1873K;

[0098] Step 3: After obtaining the smelted ingot, the alloy is homogenized in a box furnace (KSL-1800x-A1-W) in an argon protective atmosphere at a homogenization temperature of 1473K for 2 hours, followed by furnace cooling;

[0099] Step 4: cold rolling the alloy using a four-roller rolling mill, with a single rolling reduction of 20% and a total rolling reduction of 60%, to obtain an alloy sheet with a thickness of 2 mm;

[0100] Step 5: Slice the cold-rolled alloy sheet to obtain a sample with a size of 12 mm × 10 mm × 2 mm, and anneal it in a vacuum tube furnace (GSL_1600X) filled with argon at a temperature of 1300 K for 1 h to obtain an annealed alloy sheet.

[0101] Comparative Example 1

[0102] Step 1: According to the chemical formula Fe 56.5 Cr 14 Co23 W 6.5 (mass percentage) for batching, the raw materials used are blocks corresponding to the purity of each element greater than 99.90%;

[0103] Step 2: Use a vacuum induction magnetic levitation melting furnace (AM800-3, Hefei Kejing Material Technology Co., Ltd.) to melt in an argon protective atmosphere until the vacuum degree reaches 10 -3 After Pa, argon gas was filled until the pressure returned to normal slightly, the melting temperature was 1773K, the melting was repeated 4 times, and the rectangular alloy ingot was cast at 1873K;

[0104] Step 3: After obtaining the smelted ingot, the alloy is homogenized in a box furnace (KSL-1800x-A1-W) in an argon protective atmosphere at a homogenization temperature of 1473 K for 2 h, followed by furnace cooling.

[0105] Step 4: Cut a small cube from the middle of the alloy for microstructure observation and performance testing.

[0106] Test results: Fe obtained in Comparative Example 1 56.5 Cr 14 Co 23 W 6.5 The XRD spectrum of the alloy is as follows Fig.12 As shown. Fig.12 The XRD spectrum of the alloy shows a body-centered cubic (BCC) structure. The microstructure scanning electron microscope morphology and X-ray energy spectrum (EDS) surface scan, such as Fig.13 As shown, Fig.13 The image shows that the W element is evenly distributed in the Fe 61.7 Cr 15.3 Co 23.1 There is no obvious element segregation at the micron level in the alloy. Fig.14 Fe 56.5 Cr 14 Co 23 W 6.5 Alloy tensile curve. Fig.14 It can be seen that Fe 56.5 Cr 14 Co 23 W 6.5 The alloy has a yield strength of 185 MPa, a tensile strength of 978 MPa, and a uniform elongation of 13.5%. 56.5 Cr 14 Co 23 W 6.5 The resistivity of the alloy reaches 120μm·cm, and the temperature coefficient of resistance is -0.0073ppm / ℃.

[0107] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0108] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing an iron-based resistance alloy sheet based on a rolling annealing process, characterized in that: The following steps are involved: An alloy obtained by smelting and homogenizing Fe, Cr, Co and W metal materials; The alloy is composed of the following components in percentage by mass: Fe 50-60wt%, Cr 14-20wt%, Co 20-23wt%, W 4-7wt%, totaling 100%; The alloy is cold rolled with a cold rolling reduction of 10-90% to obtain a cold rolled alloy sheet; The cold-rolled alloy sheet is sliced ​​and then annealed under a protective atmosphere at 1223-1323 K. The grain size and defect density of the alloy are changed by the annealing treatment, and a face-centered cubic phase is generated to obtain an iron-based resistance alloy sheet.

2. The method for preparing an iron-based resistance alloy sheet based on a rolling annealing process according to claim 1, characterized in that: The annealing temperature is 1223K.

3. The method for preparing an iron-based resistance alloy sheet based on a rolling annealing process according to claim 1, characterized in that: The annealing time is 1-1.5h.

4. The method for preparing an iron-based resistance alloy sheet based on a rolling annealing process according to claim 3, characterized in that: The annealing time is 1h.

5. The method for preparing an iron-based resistance alloy sheet based on a rolling annealing process according to claim 1, characterized in that: The number of cold rolling times is 1-5 times, and the single pressing amount is 10-20%.

6. The method for preparing an iron-based resistance alloy sheet based on a rolling annealing process according to claim 1, characterized in that: The thickness of the alloy sheet after cold rolling is 0.5-4.5 mm.

7. The iron-based resistance alloy according to claim 4, characterized in that: The alloy consists of the following components in mass percentage: Fe 56.5wt%, Cr 14wt%, Co 23wt%, and W 6.5wt%.

8. An iron-based resistance alloy plate prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the iron-based resistance alloy plate material according to claim 8 in a patch type strain resistance sensor.

Citation Information

Patent Citations

  • Iron-aluminum-serial multielement high-resistance electrothermal alloy and preparation method thereof

    CN104087843A

  • Manufacture of alloy for strain gauge and strain gauge itself

    JP1986015914A

  • Precision electrical resistance alloy having high electrical resistance and low temperature coefficient and its manufacture

    JP1992052243A

  • High-strength and ductile multicomponent precision resistance alloys and fabrication methods thereof

    US20230257855A1