Production method of low-cost 440MPa-grade hot continuous rolled steel plate for automobile structure

By adjusting the smelting process and cooling mode, the complex and high cost of production processes for traditional automobiles is solved, and the production of low-cost and high-strength 440MPa-grade hot rolled steel plates for automobile structures is realized, simplifying the process flow and reducing the Energy consumption and meets the requirements of green manufacturing.

CN119020665AInactive Publication Date: 2024-11-26BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411086368.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The production process of traditional automotive high-strength steel plates has problems such as long process, complex process and high energy consumption. The addition of expensive alloy elements increases costs and deteriorates welding performance, making it difficult to meet green manufacturing and cost requirements.

Method used

Using a smelting process that does not require vacuum treatment, the low-cost, high-strength, hot rolled steel plate for automotive structures is produced by adjusting the thermal mechanical pressure-controlled processing (TMCP) parameters and grouped partition laminar flow cooling mode, with no chemical composition. Microalloy elements such as Nb, V, Ti, Ni, Mo, Cr control the discharge temperature and cooling speed to achieve phase change strengthening.

Benefits of technology

It has achieved low-cost and high-strength hot continuous rolled steel plate production for automotive structures, reducing production costs and energy consumption, simplifying the process flow, improving production efficiency, and in line with the development direction of green steel materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004985288990000041
    Figure BDA0004985288990000041
  • Figure BDA0004985288990000042
    Figure BDA0004985288990000042
Patent Text Reader

Abstract

The invention discloses a production method of a low-cost 440MPa-grade hot continuous rolled steel plate for an automobile structure. The production method comprises the following steps: (1) a smelting process does not need RH vacuum treatment; (2) the tapping temperature is controlled to be higher than 1080 DEG C; (3) the initial rolling temperature of an austenite recrystallization area is controlled to be larger than or equal to 1040 DEG C, the finish rolling temperature is controlled to be 830-880 DEG C, the reduction rate of the first pass of finish rolling is controlled to be 40-50%, and the reduction rate of the second pass of finish rolling is controlled to be 45-55%; (4) after hot rolling, a grouping partition type laminar cooling mode is adopted for cooling; (5) the cooling speed is controlled to be reduced to 300 DEG C or below, and then air cooling is conducted to the room temperature; (6) the thickness of the steel plate is 2.00 mm; steel sheet chemical compositions are also defined. According to the steel, microalloy elements do not need to be added on the basis of C-Mn steel, the phase change effect is fully exerted by changing the TMCP technological parameter technology, and the low-cost and high-strength hot continuous rolling steel plate for the automobile structure can be produced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgical steel rolling, and in particular relates to a method for producing a low-cost 440MPa-grade hot-rolled steel plate for automobile structure. Background Art

[0002] In recent years, my country's automobile industry has continued to develop at a high speed, which has brought great impacts on social energy supply and environmental protection. In response to environmental pressure, the state has successively issued a series of programmatic documents, clearly pointing out that my country's manufacturing industry should accelerate the pace of transformation to green manufacturing and ecological development. Existing research shows that lightweighting is the most effective measure to achieve energy conservation and emission reduction in automobiles, and high strengthening of steel materials is an important technical path to achieve lightweighting of automobiles. Greening and high performance have become the development trend of steel materials for automobiles.

[0003] Traditionally, 2.0mm thick high-strength steel plates for automobiles are produced by hot rolling + cold rolling. This method has the disadvantages of long process, complex procedures, and high energy consumption, and faces huge challenges from green manufacturing and raw material costs in the automotive industry. Therefore, a new topic has been raised for steel companies on how to adapt to market requirements and develop high-strength steel for automobiles that is both safe, energy-saving, and environmentally friendly and has high added value by replacing cold with hot. Summary of the invention

[0004] In order to improve market competitiveness, hot-rolled steel sheets often adopt a higher alloy composition design scheme to obtain ideal structural properties. For example, in order to inhibit the formation of pearlite and improve the hardenability of steel, expensive alloy elements such as Mo, Cr, Nb, Ti, and Ni are added. The addition of these elements not only increases the cost, but also deteriorates the welding performance of the steel. The purpose of the present invention is to provide a low-cost 440MPa grade hot-rolled steel sheet for automobile structure. The steel grade does not need to add micro-alloy elements on the basis of C-Mn steel. By changing the TMCP process parameter technology, the phase transformation effect is fully utilized to produce a low-cost, high-strength "hot instead of cold" hot-rolled steel sheet for automobile structure.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] The present invention provides a method for producing a low-cost 440MPa grade hot-rolled steel plate for automobile structure, comprising:

[0007] (1) The smelting process does not require RH vacuum treatment;

[0008] (2) The billet is heated in a heating furnace and the furnace temperature is controlled to be greater than 1080°C;

[0009] (3) The starting rolling temperature of the austenite recrystallization zone is controlled to be ≥1040°C, the final rolling temperature is strictly controlled at 830-880°C, the first pass of finishing rolling is controlled to have a reduction rate of 40-50%, the second pass to have a reduction rate of 45-55%, and the remaining passes are conventional reduction rates;

[0010] (4) After hot rolling, cooling is carried out in a grouped partitioned laminar cooling mode;

[0011] (5) Control the cooling rate to below 300°C, and then air cool to room temperature;

[0012] (6) Steel plate thickness 2.00 mm;

[0013] The chemical composition of the steel plate is as follows by weight percentage: 0.10-0.21% C, 0.010-0.050% Si, 0.40-1.00% Mn, P≤0.020%, S≤0.020%, Alt≥0.010%, and the rest is Fe and unavoidable inclusions.

[0014] Furthermore, the mechanical properties meet the following requirements: yield strength R eL Greater than 305MPa; tensile strength R m Greater than 440MPa; Total elongation after fracture A 50 Greater than 30%; the bending center diameter is 3 times the finished steel plate thickness, and the bending angle is 180°.

[0015] Furthermore, the chemical composition of the steel plate is as follows by weight percentage: C: 0.17%, Si: 0.030%, Mn: 0.67%, P: 0.015%, S: 0.004%, Alt: 0.030%, and the rest is Fe and unavoidable inclusions.

[0016] Furthermore, the chemical composition of the steel plate is as follows by weight percentage: C: 0.18%, Si: 0.016%, Mn: 0.63%, P: 0.013%, S: 0.007%, Alt: 0.029%, and the rest is Fe and unavoidable inclusions.

[0017] Furthermore, the chemical composition of the steel plate is as follows by weight percentage: C: 0.17%, Si: 0.020%, Mn: 0.64%, P: 0.007%, S: 0.005%, Alt: 0.021%, and the rest is Fe and unavoidable inclusions.

[0018] Furthermore, the chemical composition of the steel plate is as follows by weight percentage: C: 0.17%, Si: 0.016%, Mn: 0.63%, P: 0.009%, S: 0.006%, Alt: 0.026%, and the rest is Fe and unavoidable inclusions.

[0019] Furthermore, the chemical composition of the steel plate is as follows by weight percentage: C: 0.19%, Si: 0.0111%, Mn: 0.67%, P: 0.012%, S: 0.008%, Alt: 0.024%, and the rest is Fe and unavoidable inclusions.

[0020] Compared with the prior art, the beneficial technical effects of the present invention are:

[0021] The smelting process does not require RH treatment, and does not require the addition of micro-alloy elements such as Nb, V, Ti, Ni, Mo, and Cr, which can achieve low smelting component costs. The strength and toughness of steel are improved through phase transformation strengthening mechanism.

[0022] The application of the present invention can reduce costs, simplify production processes, improve production efficiency, reduce energy consumption and other economic and social benefits, and is in line with the development direction of developing energy-saving, clean green steel. DETAILED DESCRIPTION

[0023] The following is a further detailed description of a production method for a low-cost 440MPa grade hot-rolled steel plate for automobile structure with examples:

[0024] Table 1 lists the chemical composition of the production method of the present invention for producing a low-cost 440MPa grade hot-rolled steel plate for automobile structure. The billet thickness is 72mm and is heated in a heating furnace. The start rolling temperature and the final rolling temperature are controlled, and the steel plate is cooled after rolling to control the cooling rate. The cooling control process is shown in Table 2, and the mechanical properties are shown in Table 3. The inspection performance of the finished product meets the user requirements.

[0025] Table 1 Measured chemical composition of the examples, wt%

[0026] C Say Mn P S All 0.17 0.030 0.67 0.015 0.004 0.030 0.18 0.016 0.63 0.013 0.007 0.029 0.18 0.020 0.64 0.007 0.005 0.021 0.18 0.016 0.63 0.009 0.006 0.026 0.19 0.011 0.67 0.012 0.008 0.024

[0027] Table 2: Actual measurement of controlled rolling and controlled cooling process in the embodiment

[0028]

[0029] Table 3 Measured mechanical properties of the examples

[0030]

[0031] The embodiments described above are only descriptions of the preferred embodiments of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for producing low-cost 440MPa grade hot-rolled steel plate for automobile structure, characterized in that: include: (1) The smelting process does not require RH vacuum treatment; (2) The billet is heated in a heating furnace and the furnace temperature is controlled to be greater than 1080°C; (3) The starting rolling temperature of the austenite recrystallization zone is controlled to be ≥1040°C, the final rolling temperature is strictly controlled at 830-880°C, the first pass of finishing rolling is controlled to have a reduction rate of 40-50%, the second pass to have a reduction rate of 45-55%, and the remaining passes are conventional reduction rates; (4) After hot rolling, cooling is carried out in a grouped partitioned laminar cooling mode; (5) Control the cooling rate to below 300°C, and then air cool to room temperature; (6) Steel plate thickness 2.00 mm; The chemical composition of the steel plate is as follows by weight percentage: 0.10-0.21% C, 0.010-0.050% Si, 0.40-1.00% Mn, P≤0.020%, S≤0.020%, Alt≥0.010%, and the rest is Fe and unavoidable inclusions.

2. The method for producing low-cost 440MPa grade hot-rolled steel sheet for automobile structure according to claim 1, characterized in that: Mechanical properties meet: yield strength R eL Greater than 305MPa; tensile strength R m Greater than 440MPa; total elongation after fracture A 50 Greater than 30%; the bending center diameter is 3 times the finished steel plate thickness, and the bending angle is 180°.

3. The method for producing low-cost 440MPa grade hot-rolled steel sheet for automobile structure according to claim 1, characterized in that: The chemical composition of the steel plate is as follows by weight percentage: C: 0.17%, Si: 0.030%, Mn: 0.67%, P: 0.015%, S: 0.004%, Alt: 0.030%, and the rest is Fe and inevitable inclusions.

4. The method for producing low-cost 440MPa grade hot-rolled steel sheet for automobile structure according to claim 1, characterized in that: The chemical composition of the steel plate is as follows by weight percentage: C: 0.18%, Si: 0.016%, Mn: 0.63%, P: 0.013%, S: 0.007%, Alt: 0.029%, and the rest is Fe and inevitable inclusions.

5. The method for producing low-cost 440MPa grade hot-rolled steel sheet for automobile structure according to claim 1, characterized in that: The chemical composition of the steel plate is as follows by weight percentage: C: 0.17%, Si: 0.020%, Mn: 0.64%, P: 0.007%, S: 0.005%, Alt: 0.021%, and the rest is Fe and unavoidable inclusions.

6. The method for producing low-cost 440MPa grade hot-rolled steel sheet for automobile structure according to claim 1, characterized in that: The chemical composition of the steel plate is as follows by weight percentage: C: 0.17%, Si: 0.016%, Mn: 0.63%, P: 0.009%, S: 0.006%, Alt: 0.026%, and the rest is Fe and unavoidable inclusions.

7. The method for producing low-cost 440MPa grade hot-rolled steel sheet for automobile structure according to claim 1, characterized in that: The chemical composition of the steel plate is as follows by weight percentage: C: 0.19%, Si: 0.0111%, Mn: 0.67%, P: 0.012%, S: 0.008%, Alt: 0.024%, and the rest is Fe and unavoidable inclusions.

Citation Information

Patent Citations

  • Hot rolled steel plate for automobile structure and production method thereof

    CN103469059A

  • 440MPa-class cold-rolled high-intensity automobile structural steel and manufacturing method thereof

    CN103509997A

  • 280 Mpa grade cold-rolled strip for automobile structure and manufacturing method thereof

    CN111304540A

  • Low-cost 400MPa-grade cold-rolled continuous annealing steel strip and production method thereof

    CN113684419A

  • Production method of low-carbon manganese steel for light-weight compartment of light-weight freight vehicle

    CN116694889A