Gold plating method for tellurium-zinc-cadmium crystal

Direct depositing gold electrodes on zinc tellurium cadmium crystals through chemical wet gold plating technology solves the complex and wasteful problems of traditional physical vapor deposition technology, and realizes the preparation of gold electrodes with excellent performance, which is suitable for the manufacturing of detectors.

CN119020762APending Publication Date: 2024-11-26ANHUI PIONEER ADVANCED TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411129460.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional physical vapor deposition technology operates complexly in zinc tellurium crystal plating electrode process and wastes materials, resulting in wasting time and metal costs, making it difficult to prepare gold electrodes with excellent performance.

Method used

Using chemical wet gold plating technology, zinc tellurium cadmium crystals are soaked in the methanol solution of gold chloride, and directly deposited the gold electrodes using chemical potential energy differences, including multiple immersions in the methanol solution of bromine methanol, methanol and gold chloride. The process is made to form a dense gold electrode.

Benefits of technology

A simple and fast gold plating process is realized, and the appearance, adhesion and aging performance of the prepared gold electrode are significantly better than that of the physical vapor deposition method, and have wide application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure HDA0004997406350000011
    Figure HDA0004997406350000011
  • Figure HDA0004997406350000012
    Figure HDA0004997406350000012
Patent Text Reader

Abstract

The invention discloses a gold plating method for tellurium-zinc-cadmium crystals, which belongs to the technical field of detectors and comprises the following steps: soaking the tellurium-zinc-cadmium crystals in a bromine methanol solution; soaking the cadmium zinc telluride crystal in methanol; and then soaking and depositing the tellurium-zinc-cadmium crystal in a methanol solution of gold chloride, finally soaking with methanol, drying, and grinding to remove gold deposited on the side surface of the tellurium-zinc-cadmium crystal to finish gold plating. The cadmium zinc telluride crystal is sequentially soaked in a bromine methanol solution, methanol, a methanol solution of gold chloride and methanol, then a chemical wet gold plating process is adopted, the cadmium zinc telluride crystal is directly placed in the methanol solution of the gold chloride, gold is directly deposited on a sheet by utilizing the difference of chemical potential energy, a layer of compact gold electrode is formed, and the cadmium zinc telluride is obtained. The performance of the gold electrode prepared by adopting a wet gold plating process is obviously superior to that of the gold electrode prepared by adopting a physical vapor deposition method, and a foundation is laid for preparation of a detector.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of detectors, and in particular to a gold plating method for a cadmium zinc telluride crystal. Background Art

[0002] Cadmium zinc telluride crystal, also known as CZT in English, is a wide-bandgap II-VI compound semiconductor. With the continuous development of science and technology, the application prospects of cadmium zinc telluride crystal are becoming more and more broad. In the fields of infrared detectors, room temperature nuclear radiation detectors, etc., CZT crystals have shown important application value. At the same time, with the continuous advancement of preparation technology and the reduction of costs, the application scope of CZT crystals will be further expanded.

[0003] Currently, in the preparation field of CZT detectors, the process of electrode plating is involved. The traditional physical vapor deposition technology requires vacuuming, patching and other processes during the preparation process. The operation is complicated and wastes materials, resulting in a waste of time and metal costs.

[0004] In view of this, this application is filed. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for gold plating of cadmium zinc telluride crystals, which can quickly plate gold on the surface of the cadmium zinc telluride crystals. The prepared gold electrode has excellent appearance, adhesion and aging performance and has broad application prospects.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A gold plating method for a cadmium zinc telluride crystal comprises the following steps:

[0008] The cadmium zinc telluride crystal is immersed in a bromine methanol solution; then the cadmium zinc telluride crystal is immersed in methanol; then the cadmium zinc telluride crystal is immersed in a methanol solution of gold chloride for deposition, and finally immersed in methanol, dried, and ground to remove the gold deposited on the side of the cadmium zinc telluride crystal to complete the gold plating.

[0009] The invention soaks cadmium zinc telluride crystals in bromine methanol solution, methanol, methanol solution of gold chloride and methanol solution in sequence, then adopts a chemical wet gold plating process to directly place the cadmium zinc telluride crystals in the methanol solution of gold chloride, and directly deposits gold on a sheet by utilizing the difference in chemical potential energy to form a layer of dense gold electrode. The gold electrode prepared by the wet gold plating process has significantly better performance than that prepared by a physical vapor deposition method, thus laying a foundation for the preparation of detectors.

[0010] The method of the invention is simple and rapid. The gold chloride involved has special properties and is easily soluble in water. A chemical reaction will occur when a wafer is directly placed in a methanol solution of gold chloride, and a dense gold electrode is deposited on the surface of the wafer. The inventor of the invention has found through research that the solvent has a significant influence on the effect. The invention adopts a methanol solution of gold chloride. Compared with an aqueous solution of gold chloride and an ethanol solution of gold chloride, the appearance, adhesion and performance of the prepared gold electrode are significantly better than those of electrodes prepared by other solvents, and has broad application prospects.

[0011] As a preferred embodiment of the present invention, the bromine methanol solution is prepared from liquid bromine and methanol in a mass ratio of (1-10): (90-99).

[0012] As a preferred embodiment of the present invention, the immersion time in the bromine methanol solution is 10 to 600 s, for example, it can be 10 s, 15 s, 20 s, 30 s, 50 s, 60 s, 80 s, 100 s, 150 s, 200 s, 250 s, 300 s, 350 s, 400 s, 450 s, 500 s, 550 s, 600 s or a range consisting of any two of the values.

[0013] As a preferred embodiment of the present invention, the immersion time in the methanol solution is 5 to 30 seconds, for example, it can be 5 seconds, 6 seconds, 8 seconds, 10 seconds, 12 seconds, 15 seconds, 18 seconds, 20 seconds, 22 seconds, 25 seconds, 28 seconds, 30 seconds or a range consisting of any two of the values.

[0014] As a preferred embodiment of the present invention, the mass concentration of gold chloride in the methanol solution of gold chloride is 1-10%, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or a range consisting of any two values ​​therein.

[0015] As a preferred embodiment of the present invention, the mass concentration of gold chloride in the methanol solution of gold chloride is 3%.

[0016] As a preferred embodiment of the present invention, the immersion deposition time in the methanol solution of gold chloride is 10 to 120 s, for example, it can be 10 s, 15 s, 20 s, 30 s, 40 s, 50 s, 60 s, 70 s, 80 s, 90 s, 100 s, 110 s, 120 s or a range consisting of any two of the values.

[0017] As a preferred embodiment of the present invention, the immersion deposition time in the methanol solution of gold chloride is 60 seconds.

[0018] As a preferred embodiment of the present invention, the time for immersion treatment with methanol is 5 to 30 seconds, for example, it can be 5 seconds, 6 seconds, 8 seconds, 10 seconds, 12 seconds, 15 seconds, 18 seconds, 20 seconds, 22 seconds, 25 seconds, 28 seconds, 30 seconds or a range consisting of any two values ​​therein.

[0019] The beneficial effects of the present invention are as follows: (1) The present invention sequentially soaks cadmium zinc telluride crystals with bromine methanol solution, methanol solution, gold chloride methanol solution, and methanol solution, and then uses a chemical wet gold plating process to directly place the cadmium zinc telluride crystals in a gold chloride methanol solution, and utilizes the difference in chemical potential energy to directly deposit gold on the wafer to form a layer of dense gold electrode. The performance of the gold electrode prepared by the wet gold plating process of the present invention is significantly better than that prepared by the physical vapor deposition method, which lays a foundation for the preparation of the detector. (2) The method of the present invention is simple and fast, and the gold chloride involved has special properties and is easily soluble in water. Placing the wafer directly in the gold chloride methanol solution will produce a chemical reaction, and a dense gold electrode will be deposited on the surface of the wafer. The inventor of the present invention has found that the solvent has a significant effect on the effect. The present invention uses a methanol solution of gold chloride. Compared with an aqueous solution of gold chloride and an ethanol solution of gold chloride, the appearance, adhesion and performance of the gold electrode prepared by the present invention are significantly better than the performance of electrodes prepared by other solvents, and has a wide range of application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the appearance of the electrodes prepared in Example 1 and Comparative Example 3.

[0021] Figure 2 The following are the appearance pictures of the electrodes prepared in Example 1 and Comparative Example 3 after aging.

[0022] Figure 3 The following are appearance diagrams of the electrodes prepared in Example 1, Comparative Example 1, and Comparative Example 2.

[0023] Figure 4 The following are appearance pictures of the electrodes prepared in Example 1, Comparative Example 1 and Comparative Example 2 after aging. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0025] In this application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions of the listed features.

[0026] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0027] In the present application, there is no particular limitation on the specific dispersion and stirring treatment methods.

[0028] Unless otherwise specified, the components, raw materials or instruments used in the embodiments and comparative examples of the present invention are all commercially available raw materials or instruments, and the components and raw materials used in each parallel experiment are all of the same kind.

[0029] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0030] The following examples are provided to facilitate understanding of the present invention. These examples are not provided to limit the scope of the claims.

[0031] Example 1

[0032] A gold plating method for a cadmium zinc telluride crystal comprises the following steps:

[0033] (1) placing the cadmium zinc telluride crystal in a bromine methanol solution (prepared with liquid bromine and methanol in a mass ratio of 5:95) for immersion for 120 seconds;

[0034] (2) soaking the cadmium zinc telluride crystal in methanol for 20 seconds;

[0035] (3) then immersing the cadmium zinc telluride crystal in a methanol solution with a mass concentration of 3% gold chloride for deposition for 60 seconds;

[0036] (4) Finally, the CdZnTe crystal is immersed in methanol for 60 seconds, dried, and ground to remove the gold deposited on the side of the CdZnTe crystal to complete the gold plating.

[0037] Example 2

[0038] A gold plating method for a cadmium zinc telluride crystal comprises the following steps:

[0039] (1) placing the cadmium zinc telluride crystal in a bromine methanol solution (prepared with liquid bromine and methanol in a mass ratio of 5:95) for immersion for 120 seconds;

[0040] (2) soaking the cadmium zinc telluride crystal in methanol for 20 seconds;

[0041] (3) then immersing the CdZnTe crystal in a methanol solution with a mass concentration of 10% gold chloride for deposition for 20 seconds;

[0042] (4) Finally, the CdZnTe crystal is immersed in methanol for 60 seconds, dried, and ground to remove the gold deposited on the side of the CdZnTe crystal to complete the gold plating.

[0043] Example 3

[0044] A gold plating method for a cadmium zinc telluride crystal comprises the following steps:

[0045] (1) placing the cadmium zinc telluride crystal in a bromine methanol solution (prepared with liquid bromine and methanol in a mass ratio of 5:95) for immersion for 120 seconds;

[0046] (2) soaking the cadmium zinc telluride crystal in methanol for 20 seconds;

[0047] (3) then immersing the CdZnTe crystal in a methanol solution with a mass concentration of 1% gold chloride for deposition for 120 seconds;

[0048] (4) Finally, the CdZnTe crystal is immersed in methanol for 60 seconds, dried, and ground to remove the gold deposited on the side of the CdZnTe crystal to complete the gold plating.

[0049] Comparative Example 1

[0050] A gold plating method for a cadmium zinc telluride crystal comprises the following steps:

[0051] (1) placing the cadmium zinc telluride crystal in a bromine methanol solution (prepared with liquid bromine and methanol in a mass ratio of 5:95) for immersion for 120 seconds;

[0052] (2) soaking the cadmium zinc telluride crystal in methanol for 20 seconds;

[0053] (3) then immersing the cadmium zinc telluride crystal in an aqueous solution with a mass concentration of 3% gold chloride for deposition for 60 seconds;

[0054] (4) Finally, the CdZnTe crystal is immersed in methanol for 60 seconds, dried, and ground to remove the gold deposited on the side of the CdZnTe crystal to complete the gold plating.

[0055] Comparative Example 2

[0056] A gold plating method for a cadmium zinc telluride crystal comprises the following steps:

[0057] (1) placing the cadmium zinc telluride crystal in a bromine methanol solution (prepared with liquid bromine and methanol in a mass ratio of 5:95) for immersion treatment for 120 seconds;

[0058] (2) soaking the cadmium zinc telluride crystal in methanol for 20 seconds;

[0059] (3) then immersing the cadmium zinc telluride crystal in an ethanol solution with a mass concentration of 3% gold chloride for deposition for 60 seconds;

[0060] (4) Finally, the CdZnTe crystal is immersed in methanol for 60 seconds, dried, and ground to remove the gold deposited on the side of the CdZnTe crystal to complete the gold plating.

[0061] Comparative Example 3

[0062] The difference between Comparative Example 3 and Example 1 is that in Comparative Example 3, after the CdZnTe crystal is cleaned and dried with nitrogen, gold having the same thickness as that in Example 1 is plated on the surface of the CdZnTe crystal by a magnetron sputtering method.

[0063] Test Case

[0064] 1. As Figure 1 As shown, the appearance of the cadmium zinc telluride crystals prepared by the wet gold plating of Example 1 and Comparative Example 3 is not much different, and the color of the wet gold plating sample is relatively light.

[0065] 2. The wet gold plating method of Example 1 ( Figure 2 The top four, the rightmost crystal was not tested) and Comparative Example 3 ( Figure 2 The four crystals below (the rightmost crystal was not tested) were aged for 24 hours in an environment with a temperature of 85°C and a humidity of 85 degrees, and then the adhesion was tested with 3M tape (the 3M tape was pasted on the surface of the CdZnTe crystal, left to stand for a few seconds, and then torn off to observe whether the gold electrode on the CdZnTe crystal was taken off together. If so, it proves that the electrode adhesion is poor. If the electrode is intact, it proves that the electrode adhesion is good.). Figure 2 As shown, there is almost no gold loss in the wet gold plating after the aging test, which proves that the adhesion of the wet gold plating sample is faster and better than the usual electrode preparation method.

[0066] The leakage current before and after aging is shown in Table 1.

[0067]

[0068] It can be clearly seen from the table that the leakage current of wet gold plating is significantly lower than that of magnetron gold plating, which proves that the performance of wet gold plating is better than that of magnetron gold plating. After the sample is aged, the leakage current of the wet plated electrode remains within 10 nanoamperes, which is significantly better than the performance of the magnetron sputtering electrode after aging.

[0069] 3. Example 1, Comparative Examples 1-2 Soaking the Deposited Electrodes in Different Solvents Figure 3 As shown, the electrode immersed in the methanol solution of gold chloride has a lighter color, the electrode immersed in the aqueous solution of gold chloride has a darker color, and the electrode immersed in the ethanol solution of gold chloride has a yellower color. It can be seen that the appearance of the electrode immersed in the methanol solution of gold chloride is better.

[0070] 4. The electrodes prepared in Example 1 and Comparative Examples 1 to 2 were aged for 24 hours in an environment of a temperature of 85°C and a humidity of 85 degrees to obtain the results shown in the figure. The color of the electrodes plated with an aqueous solution of gold chloride became darker, while the color of the electrodes plated with methanol solvent and ethanol solvent had almost no change.

[0071] The adhesion of electrodes plated under three conditions was tested with 3M tape. The results showed that large pieces of gold chloride-plated electrodes in the aqueous solution of gold chloride and the ethanol solution of gold chloride fell off, while only the edges of gold chloride-plated electrodes in the methanol solution of gold chloride fell off, proving that the methanol solution of gold chloride has the best adhesion.

[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for gold plating of cadmium zinc telluride crystals, characterized in that: The following steps are involved: The cadmium zinc telluride crystal is immersed in a bromine methanol solution; then the cadmium zinc telluride crystal is immersed in methanol; then the cadmium zinc telluride crystal is immersed in a methanol solution of gold chloride for deposition, and finally immersed in methanol, dried, and ground to remove the gold deposited on the side of the cadmium zinc telluride crystal to complete the gold plating.

2. The gold plating method of CdZnTe crystal according to claim 1, characterized in that: The bromine methanol solution is prepared from liquid bromine and methanol in a mass ratio of (1-10): (90-99).

3. The gold plating method of CdZnTe crystal according to claim 1, characterized in that: The bromine methanol solution is prepared by mixing liquid bromine and methanol in a mass ratio of 5:

95.

4. The gold plating method of CdZnTe crystal according to claim 1, characterized in that: The soaking time in the bromine methanol solution is 10 to 600 seconds.

5. The gold plating method of CdZnTe crystal according to claim 1, characterized in that: The immersion time in methanol is 5 to 30 seconds.

6. The gold plating method of CdZnTe crystal according to claim 1, characterized in that: The mass concentration of gold chloride in the gold chloride methanol solution is 1-10%.

7. The gold plating method of CdZnTe crystal according to claim 1, characterized in that: The mass concentration of gold chloride in the gold chloride methanol solution is 3%.

8. The gold plating method of CdZnTe crystal according to claim 1, characterized in that: The immersion deposition time in the methanol solution of gold chloride is 10 to 120 seconds.

9. The gold plating method of CdZnTe crystal according to claim 1, characterized in that: The immersion deposition time in the methanol solution of gold chloride is 60 seconds.

10. The gold plating method of CdZnTe crystal according to claim 1, characterized in that: The immersion time in methanol is 5 to 30 seconds.