Transition metal composite carbon-based material and application thereof in electrocatalysis of CO2
By converting corn stalks into functionalized carbon-based materials and compounding with transition metals, it is used for electrocatalytic CO2 reduction, and the problems of agricultural waste treatment and CO2 capture are solved, efficient and environmentally friendly electrocatalytic performance is achieved, and energy and Sustainable development in the field of environment.
Patent Information
- Application Number
- CN202411136157.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
The existing technology is difficult to effectively treat and utilize agricultural waste corn stalks, and lacks efficient and environmentally friendly CO2 capture and storage solutions, affecting environmental protection and sustainable development.
Through high-temperature pyrolysis technology, corn stalks are converted into functionalized biomass carbon-based materials and are combined with transition metals for electrocatalytic CO2 reduction, and a transition metal composite carbon-based materials are prepared for electrocatalytic CO2 capture and storage. .
The resource utilization of agricultural waste has been realized, the negative environmental impact has been reduced, and new impetus has been provided in the development of energy and environmental fields, with mild reaction conditions, low energy consumption and good electrocatalytic performance.
Smart Images

Figure CN119020802A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrocatalytic materials, and in particular to a transition metal composite carbon-based material and its electrocatalytic CO2 application. Background Art
[0002] Environmental problems such as climate change and sea level rise caused by increased CO2 emissions are becoming increasingly serious. It is imperative to find effective ways to manage and utilize CO2 and achieve the goal of "carbon neutrality" as soon as possible. At present, people have proposed a variety of CO2 emission reduction and utilization solutions, such as the use of carbon capture and storage technology, electrochemical CO2 reduction technology, etc. Among these technologies, it is generally believed that the use of carbon-based materials for CO2 adsorption, conversion and storage is a promising treatment method.
[0003] As far as the current distribution of crop planting in my country is concerned, the proportion of corn production in cereals has remained above 40% for ten consecutive years, and has shown an upward trend year by year. According to incomplete statistics, about 231 million tons of corn stalks will be harvested in 2023. However, the current treatment method for corn stalks still uses the traditional incineration method or straw return to the field treatment. Therefore, it is particularly important to explore new, efficient and environmentally friendly methods for corn stalk resource treatment. Studies have found that corn stalks are rich in cellulose components, and the sponge-shaped stalk core inside presents a highly cross-linked three-dimensional skeleton structure. Therefore, corn stalks can be used as a precursor of biomass carbon, which helps to construct functionalized carbon-based materials with a porous structure. In addition, the higher silicate content of corn stalks can also effectively improve the thermal stability and corrosion resistance of carbon-based materials. In summary, the development of functionalized carbon-based materials derived from corn stalks is expected to achieve further improvement in electrochemical performance.
[0004] At present, finding efficient and sustainable resource utilization and application treatment methods for straw-like agricultural waste has become one of the current research focuses. Making full use of straw-like agricultural waste, through proper treatment and transformation, to construct carbon-based materials with special functions for CO2 capture, conversion and storage, thereby promoting the development and utilization of clean energy. In this context, studying the preparation methods of functionalized agricultural waste carbon-based materials is of great significance for solving environmental problems and promoting sustainable development. Summary of the invention
[0005] The purpose of the present invention is to convert natural waste corn stalks into functionalized biomass carbon-based electrocatalytic materials through high-temperature pyrolysis technology, and apply them to the field of electrocatalytic CO2 reduction. The invention realizes the conversion of agricultural waste into efficient and environmentally friendly biomass carbon-based materials for application in the field of electrocatalysis, reduces the negative impact of agricultural waste on the environment, realizes the resource utilization of waste, provides new impetus for the development of energy and environmental fields, and has important research significance and practical value for promoting sustainable development, promoting environmental protection and the progress of new energy technologies.
[0006] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing a transition metal composite carbon-based material, comprising the following preparation steps:
[0007] (1) First, a certain amount of corn stalks are ball-milled, crushed, and sieved to form uniform small particle powder;
[0008] (2) Weighing a certain amount of uniform small particle powder and a certain amount of deionized water for ultrasonic dispersion to form a uniform mixed liquid;
[0009] (3) washing the mixture several times and freeze-drying to obtain clean corn stalk powder;
[0010] (4) Weigh clean corn stalk powder, a certain amount of transition metal salt, melamine and deionized water, and stir to form a uniform mixture for 20-30 min at a stirring speed of 150 rpm;
[0011] (5) stirring the uniform mixed liquid in an oil bath and then drying it in an oven to obtain a straw mixture;
[0012] (6) placing the straw mixture in a tube furnace and calcining it at high temperature to obtain a biomass carbon-based precursor;
[0013] (7) The biomass carbon powder is dispersed in a certain amount of hydrochloric acid and fully stirred, centrifuged and washed until neutral, and then placed in an oven for drying to finally obtain a transition metal composite carbon-based material.
[0014] Furthermore, in the step (1), the amount of corn stalks used is 400-500 g; the ball milling time is 30-60 min; and the sieve size is 100-200 mesh.
[0015] Furthermore, in the step (2), the amount of uniform small particle powder is 400-500 g; the amount of deionized water is 1-1.5 L; the ultrasonic time is 2-3 h, and the power is 40 kHz.
[0016] Furthermore, in the step (3), the washing times are 10-20 times; the washing method is: suction filtration; the washing solution is: deionized water; the freeze-drying temperature is: -45°C; and the freeze-drying time is 24-48h.
[0017] Furthermore, in the step (4), the amount of corn stalk powder is 1.5-2 g; the type of metal salt is any one of nickel nitrate, nickel sulfate or nickel chloride, and the amount thereof is 5-6 mmol; the amount of melamine is 7-8 mmol; the amount of deionized water is 100-150 mL; the stirring time is 20-30 min, and the stirring speed is 150 rpm.
[0018] Furthermore, in step (5), the temperature of the oil bath treatment is 80-90°C; the time of the oil bath treatment is 10-12h; the stirring speed is 100rpm; the temperature of the oven is 80-100°C; and the drying time is 24-48h.
[0019] Furthermore, in step (6), the calcination temperature in the tubular furnace is 800° C., the calcination time is 2 h, and the calcination atmosphere is N 2 .
[0020] Furthermore, in step (7), the hydrochloric acid concentration is 2-3M; the amount of hydrochloric acid used is: 50-100mL; the stirring time is: 24-48h; the stirring speed is 150rpm; the washing solvent is: deionized water and anhydrous ethanol for washing twice respectively; the oven temperature is: 80°C; and the drying time is 24-48h.
[0021] Furthermore, the transition metal composite carbon-based material prepared by the preparation method described in any one of claims 1 to 8 is used for electrocatalysis of CO2.
[0022] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0023] The present invention utilizes waste biomass corn stalks to produce electrocatalytic CO2 reduction electrode materials, realizing waste resource utilization while providing new impetus for the development of energy and environmental fields. The present invention has the characteristics of mild reaction conditions, short reaction time, low energy consumption, and environmental friendliness, is suitable for mass production, and has certain application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0025] Figure 1 The SEM images of the transition metal composite carbon-based materials in Examples 1, 2, and 3.
[0026] Figure 2 TEM spectra of the transition metal composite carbon-based materials in Examples 1, 2, and 3.
[0027] Figure 3 This is the EDS-mapping spectrum of the transition metal composite carbon-based materials in Examples 1, 2, and 3.
[0028] Figure 4 1 is the XRD spectrum of the transition metal composite carbon-based material in Examples 1, 2 and 3.
[0029] Figure 5 The linear sweep voltammetry curves of the transition metal composite carbon-based materials in Examples 1, 2, and 3 and the Faraday efficiency spectra of CO and H2. DETAILED DESCRIPTION
[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0031] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of a transition metal composite carbon-based material prepared in the following examples are as follows:
[0032] The morphology of the prepared samples was observed using a JSM-7800F emission field scanning electron microscope (SEM) equipped with an energy dispersive X-ray spectrometer. The working voltage was 20 kV and the working distance was 11-13 mm.
[0033] The structure test of the prepared samples was carried out on a German Bruker D8 X-ray diffractometer (Cu-Kα radiation, The range is 10°-80°), and the scanning rate is 7°min -1 .
[0034] Electrocatalytic activity test: The electrocatalytic carbon dioxide reduction performance test of the synthesized samples was carried out in an electrochemical workstation model CHI660 produced by Shanghai Chenhua Company.
[0035] Example 1
[0036] Weigh 500g corn stalks, ball mill for 30min, crush, sieve (200 mesh), then mix the collected uniform small particle powder with 1L deionized water, and form a uniform mixture after ultrasonic treatment at 40kHz power for 2h; then, use deionized water for suction filtration and washing; finally, spread it evenly on a surface dish, freeze-dry it at -45℃ for 24h to obtain clean corn stalk powder; weigh 1.5g washed and dried corn stalk powder, 5mmol nickel nitrate and 7mmol melamine, add them to 100mL deionized water, stir to form a uniform mixture, the stirring time is 20min, and the stirring speed is 150rpm; then the mixture is The liquid was stirred in an oil bath at 80°C for 10 hours at a stirring speed of 100 rpm, and then the mixture was moved into an oven at 80°C to evaporate the water for 24 hours; thereafter, the dried straw mixture was placed in a tubular furnace and calcined at 800°C under nitrogen conditions for 2 hours to form biomass carbon powder; and the prepared biomass carbon powder was dispersed in 2M hydrochloric acid and stirred for 12 hours at a stirring speed of 150 rpm to wash away impurities therein, and then washed twice with deionized water and ethanol in sequence, washed to neutrality, and then placed in an oven at 80°C to dry for 24 hours to obtain a transition metal Ni-composite biomass carbon-based material (Ni / N-BC).
[0037] Example 2
[0038] Weigh 500g corn stalks, ball mill for 30min, crush, sieve (200 mesh), then mix the collected uniform small particle powder with 1L deionized water, and form a uniform mixture after ultrasonic treatment at 40kHz power for 2h; then, use deionized water for suction filtration and washing; finally, spread it evenly on a surface dish, freeze-dry it at -45℃ for 24h to obtain clean corn stalk powder; weigh 1.5g washed and dried corn stalk powder, 5mmol ferric nitrate and 7mmol melamine, add them to 100mL deionized water, stir to form a uniform mixture, the stirring time is 25min, and the stirring speed is 150rpm; then mix The liquid was stirred in an oil bath at 80°C for 10 hours at a stirring speed of 100 rpm, and then the mixture was moved into an oven at 80°C to evaporate the water for 36 hours; thereafter, the dried straw mixture was placed in a tubular furnace and calcined at 800°C under nitrogen conditions for 2 hours to make it into biomass carbon powder; and the prepared biomass carbon powder was dispersed in 2M hydrochloric acid and stirred for 12 hours at a stirring speed of 150 rpm to wash away the impurities therein, and then washed twice with deionized water and ethanol in sequence, washed to neutrality, and then placed in an oven at 80°C to dry for 36 hours, to obtain a transition metal Fe composite biomass carbon-based material (Fe / N-BC).
[0039] Example 3
[0040] Weigh 500g corn stalks, ball mill for 30min, crush, sieve (200 mesh), then mix the collected uniform small particle powder with 1L deionized water, and form a uniform mixture after ultrasonic treatment at 40kHz power for 2h; then, use deionized water for suction filtration and washing; finally, spread it evenly on a surface dish, freeze-dry it at -45℃ for 24h to obtain clean corn stalk powder; weigh 1.5g washed and dried corn stalk powder, 5mmol cobalt nitrate and 7mmol melamine, add them to 100mL deionized water, stir to form a uniform mixture, the stirring time is 30min, and the stirring speed is 150rpm; then mix The liquid was stirred in an oil bath at 80°C for 10 hours at a stirring speed of 100 rpm, and then the mixture was moved into an oven at 80°C to evaporate the water for 48 hours; thereafter, the dried straw mixture was placed in a tubular furnace and calcined at 800°C under nitrogen conditions for 2 hours to form biomass carbon powder; and the prepared biomass carbon powder was dispersed in 2M hydrochloric acid and stirred for 12 hours at a stirring speed of 150 rpm to wash away impurities therein, and then washed twice with deionized water and ethanol in sequence, washed to neutrality, and then placed in an oven at 80°C to dry for 48 hours to obtain a transition metal Co composite biomass carbon-based material Co / N-BC).
[0041] Effect example
[0042] like Figure 1 As shown, in Examples 1, 2, and 3, the sample morphology was characterized by scanning electron microscopy (SEM), and it can be clearly observed that the carbonized corn stalks present a unique honeycomb void structure, which provides a good carrier platform for the anchoring of metal particles. In the SEM image, it can also be observed that a large number of protruding particles are attached to the surface of the biomass carbon carrier, which are the loaded metal particles.
[0043] like Figure 2 As shown, the transmission electron microscopy (TEM) characterization of Examples 1, 2, and 3 shows that there are obvious metal particles in the transition metal composite carbon-based materials.
[0044] like Figure 3 As shown, the EDS-mapping element mapping spectra of Examples 1, 2, and 3 show that N and O elements are evenly distributed on the carbon carrier, among which the sparsely distributed metal elements (Fe, Co, Ni) indicate the heterogeneous loading of the metal components on the biomass carbon carrier.
[0045] like Figure 4 As shown, in Examples 1, 2, and 3, characteristic peaks of metal and carbon appear, proving the successful introduction of metal.
[0046] like Figure 5 As shown, the Faraday efficiency tests of the electrocatalytic carbon dioxide reduction of Examples 1, 2, and 3 indicate that the corn straw composite transition metal carbon-based material has excellent electrocatalytic carbon dioxide reduction performance.
[0047] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a transition metal composite carbon-based material, characterized in that: The method comprises the following preparation steps: (1) First, a certain amount of corn stalks are ball-milled, crushed, and sieved to form uniform small particle powder; (2) Weighing a certain amount of uniform small particle powder and a certain amount of deionized water for ultrasonic dispersion to form a uniform mixed liquid; (3) washing the mixture several times and freeze-drying to obtain clean corn stalk powder; (4) Weighing clean corn stalk powder, a certain amount of transition metal salt, melamine and deionized water, and stirring to form a uniform mixed solution; (5) stirring the uniform mixed liquid in an oil bath and then drying it in an oven to obtain a straw mixture; (6) placing the straw mixture in a tube furnace and calcining it at high temperature to obtain a biomass carbon-based precursor; (7) The biomass carbon powder is dispersed in a certain amount of hydrochloric acid and fully stirred, centrifuged and washed until neutral, and then placed in an oven for drying to finally obtain a transition metal composite carbon-based material.
2. The method for preparing a transition metal composite carbon-based material according to claim 1, characterized in that: In the step (1), the amount of corn stalks used is 400-500 g; the ball milling time is 30-60 min; and the sieve size is 100-200 mesh.
3. The method for preparing a transition metal composite carbon-based material according to claim 1, characterized in that: In the step (2), the amount of uniform small particle powder is 400-500 g; the amount of deionized water is 1-1.5 L; the ultrasonic time is 2-3 h, and the power is 40 kHz.
4. The method for preparing a transition metal composite carbon-based material according to claim 1, characterized in that: In the step (3), the washing times are 10-20 times; the washing method is suction filtration; the washing solution is deionized water; the freeze-drying temperature is -45°C; and the freeze-drying time is 24-48 hours.
5. The method for preparing a transition metal composite carbon-based material according to claim 1, characterized in that: In the step (4), the amount of corn stalk powder is 1.5-2 g; the type of metal salt is any one of nickel nitrate, nickel sulfate or nickel chloride, and the amount thereof is 5-6 mmol; the amount of melamine is 7-8 mmol; the amount of deionized water is 100-150 mL; the stirring time is 20-30 min, and the stirring speed is 150 rpm.
6. The method for preparing a transition metal composite carbon-based material according to claim 1, characterized in that: In the step (5), the temperature of the oil bath treatment is 80-90°C; the time of the oil bath treatment is 10-12h; the stirring speed is 100rpm; the temperature of the oven is 80-100°C; and the drying time is 24-48h.
7. The method for preparing a transition metal composite carbon-based material according to claim 1, characterized in that: In the step (6), the calcination temperature in the tubular furnace is 800° C., the calcination time is 2 h, and the calcination atmosphere is N2.
8. The method for preparing a transition metal composite carbon-based material according to claim 1, characterized in that: In the step (7), the hydrochloric acid concentration is 2-3M; the amount of hydrochloric acid used is: 50-100 mL; the stirring time is: 24-48 h; the stirring speed is 150 rpm; the washing solvent is: deionized water and anhydrous ethanol for washing twice respectively; the oven temperature is: 80°C; and the drying time is 24-48 h.
9. Use of the transition metal composite carbon-based material prepared by the preparation method according to any one of claims 1 to 8 for electrocatalysis of CO2.