Method for preparing lead-zinc alloy by using lead-zinc-ammonia-chlorine complex system
The lead-zinc ammonia chlorine complex system is electrolyzed under conditions without ammonia water and ammonia gas, and the problems of complex purification processes and ammonia pollution in the production of lead-zinc alloys are solved, and the process and environmental protection effects are simplified, and different proportions are generated. Lead-zinc alloy.
Patent Information
- Application Number
- CN202411098308.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-26
AI Technical Summary
The purification process in the existing lead-zinc alloy production process is complex and the ammonia-ammonium salt method will evaporate ammonia, polluting the environment.
The lead-zinc ammonia chlorine complex system is adopted, and the lead-zinc ammonia chlorine complex solution is leached under conditions of no ammonia water and no ammonia gas to obtain the lead-zinc ammonia chlorine complex solution, and electrolytic treatment is carried out in the electrolytic device to generate Lead-zinc alloy simplifies the purification process and avoids the release of ammonia.
The purification steps in the production of lead-zinc alloys are simplified, the ammonia pollution is reduced, the working environment quality is improved, and alloys with different lead-zinc ratios can be generated according to electrolytic conditions to meet industrial needs.
Smart Images

Figure CN119020825A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrometallurgy, and in particular relates to a method for preparing a lead-zinc alloy using a lead-zinc ammonia-chlorine complex system. Background Art
[0002] Lead and zinc are non-ferrous metals with similar properties and are widely used in the industrial field. With the gradual depletion of high-grade lead-zinc oxide and lead-zinc sulfide ores that are easy to beneficiate, the utilization of secondary lead-zinc materials is gradually gaining attention. There are many types of secondary lead-zinc materials, including arc furnace slag, secondary lead-zinc smoke collected by fuming furnaces, waste batteries and waste printed circuit boards. Under the national policy background of energy conservation, emission reduction and green environmental protection, taking appropriate methods to recover valuable metals from waste secondary lead-zinc materials has become a new direction of industrial development.
[0003] At present, the production method of lead-zinc alloy is that most enterprises first prepare high-purity zinc powder and lead powder, and then carry out pyrometallurgical smelting under high temperature conditions, which consumes a lot of energy. The rest of the enterprises first use hydrometallurgical processes to produce single lead and zinc metals, and then use alloying processes to prepare lead-zinc alloys. Hydrometallurgy mostly uses electrolysis to produce metallic lead or metallic zinc, but these processes all have obvious shortcomings.
[0004] The current production process of lead-zinc alloys mainly has the problem that a complex purification process is generally required before electrodeposition of metal. Although the purification process of the ammonia-ammonium salt method is relatively simple, ammonia gas will continue to volatilize during the production process, polluting the working environment. Summary of the invention
[0005] Therefore, in order to overcome some defects and shortcomings in the prior art, an embodiment of the present invention provides a method for preparing lead-zinc alloy using a lead-zinc ammonia-chlorine complex system to solve the problem of complex purification steps in the current lead-zinc alloy production process and the defect of continuous volatilization of ammonia gas during the ammonia-ammonium salt production process.
[0006] The embodiment of the present invention provides a method for preparing a lead-zinc alloy by using a lead-zinc ammonia-chlorine complex system, comprising: obtaining a lead-zinc material; adding ammonium chloride to water to prepare an ammonium chloride solution, and during the preparation process, no ammonia water is added and no ammonia gas is introduced; sending the lead-zinc material and the ammonium chloride solution to a leaching device for leaching to obtain a lead-zinc ammonia-chlorine complex solution, and during the leaching process, no ammonia water is added and no ammonia gas is introduced; placing the lead-zinc ammonia-chlorine complex solution into an electrolysis device for electrolysis treatment to generate a lead-zinc alloy at the cathode of the electrolysis device, wherein the lead-zinc alloy is a first lead-zinc alloy, or the lead-zinc alloy includes the first lead-zinc alloy and a second lead-zinc alloy.
[0007] In one embodiment of the present invention, the lead content in the lead-zinc-ammonia-chloride complex solution is greater than or equal to 0.1 mol / L, the zinc content in the lead-zinc-ammonia-chloride complex solution is greater than or equal to 0.7 mol / L, and the ammonium chloride content in the lead-zinc-ammonia-chloride complex solution is greater than or equal to 3.0 mol / L.
[0008] In one embodiment of the present invention, the control conditions of the electrolysis treatment include electrolysis temperature and current density, wherein the electrolysis temperature is 70-90°C, and the current density is 200-500A / m 2 .
[0009] In one embodiment of the present invention, the control conditions of the electrolytic treatment also include electrodeposition time, and the electrodeposition time includes a first electrodeposition time and a second electrodeposition time; when the electrodeposition time is the first electrodeposition time, the lead-zinc alloy is a first lead-zinc alloy; when the electrodeposition time is the second electrodeposition time, the lead-zinc alloy includes a first lead-zinc alloy and a second lead-zinc alloy.
[0010] In one embodiment of the present invention, the first electrodeposition time is less than or equal to 45 minutes; the second electrodeposition time is greater than or equal to 60 minutes.
[0011] In one embodiment of the present invention, the first lead-zinc alloy is a high-lead and low-zinc alloy, and the second lead-zinc alloy is a high-zinc and low-lead alloy.
[0012] In one embodiment of the present invention, the electrolysis device comprises an electrolytic cell, the electrolytic cell is provided with the cathode and the anode, and the electrolytic cell is a polyvinyl chloride electrolytic cell.
[0013] In one embodiment of the present invention, the cathode is a titanium plate, and the anode is a ruthenium-coated titanium mesh.
[0014] In one embodiment of the present invention, before the lead-zinc-ammonia-chloride complex solution is placed in the electrolytic cell for the electrolytic treatment, the process includes: adding an electrodeposition additive to the lead-zinc-ammonia-chloride complex solution to obtain a lead-zinc-ammonia-chloride complex solution to which the electrodeposition additive is added.
[0015] In one embodiment of the present invention, the electrodeposition additive is bone glue, and the dosage of the electrodeposition additive is 10-50 mg / L.
[0016] It can be seen from the above that the above technical solution has at least one or more of the following beneficial effects:
[0017] (1) The present invention prepares an ammonium chloride solution by adding ammonium chloride to water, and feeds the lead-zinc material and the ammonium chloride solution into a leaching device for leaching to obtain a lead-zinc ammonia-chloride complex solution, and then feeds the lead-zinc ammonia-chloride complex solution into an electrolytic device as an electrolyte for electrolytic treatment, and directly deposits on a cathode to form a lead-zinc alloy. Since the lead-zinc ammonia-chloride complex solution is directly used for electrolysis as an electrolyte, no complicated purification process is required, thereby simplifying the multi-step purification process required in the traditional electrolysis method. In the process flow of the present invention, the ammonium chloride solution is prepared under the condition of no ammonia water and no ammonia gas, and the lead-zinc material and the ammonium chloride solution are fed into a leaching device for leaching under the condition of no ammonia water and no ammonia gas, thereby avoiding the release of ammonia gas during the production process, thereby effectively reducing the pollution to the working environment, improving the air quality in the workplace, and protecting the health of employees. In addition, by controlling the conditions of the electrolytic treatment, the present invention can generate alloys with different lead-zinc ratios according to the needs of specific applications, thereby meeting the specific requirements of different industrial fields for material properties.
[0018] (2) The present invention uses a lead-zinc ammonia-chlorine complex solution as an electrolyte and places it in an electrolytic cell for electrolysis. The electrolytic cell can control the temperature of the electrolyte so that the temperature of the leaching solution is moderate. In addition, the pH of the leaching solution is nearly neutral, which has the advantage of not being easy to corrode equipment. In addition, due to the strong selectivity of ammonia and chlorine in the lead-zinc ammonia-chlorine complex solution, the electrolyte can be directly put into electrolysis without going through a complicated purification step, thereby simplifying the operation steps. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0020] Figure 1 The present invention provides a schematic flow chart of a method for preparing a lead-zinc alloy using a lead-zinc ammonia-chlorine complex system.
[0021] Figure 2 for Figure 1 Schematic diagram of the process of the additional steps before step S40.
[0022] Figure 3 This is a macroscopic morphology of a high-lead, low-zinc alloy prepared in a specific embodiment of the present invention.
[0023] Figure 4 This is a macroscopic morphology of a high-zinc and low-zinc lead alloy prepared in a specific embodiment of the present invention.
[0024] Figure 5 The figure is a curve diagram showing the variation of the metal recovery rate at the cathode of the electrolytic cell with the electrolysis time in a specific embodiment of the present invention.
[0025] Figure 6a This is a scanning electron microscope (SEM) image of the morphology of the high-lead, low-zinc alloy prepared in a specific embodiment of the present invention.
[0026] Figure 6b to Figure 6f The nitrogen, oxygen, lead, chlorine and zinc elements in the high-lead and low-zinc alloy in the specific embodiment of the present invention are Figure 6a Element distribution area diagram in the SEM photograph shown.
[0027] Figure 6g This is a diagram of the electron radiation intensity of nitrogen, oxygen, lead, chlorine and zinc in the high-lead and low-zinc alloy in a specific embodiment of the present invention.
[0028] Figure 6h This is a data diagram of the weight percentage and atomic percentage of each element on the surface of the high-lead, low-zinc alloy in a specific embodiment of the present invention.
[0029] Figure 7a This is a scanning electron microscope (SEM) image of the morphology of the high-zinc and low-lead alloy prepared in a specific embodiment of the present invention.
[0030] Figure 7b to Figure 7f 1 is an element distribution area diagram of nitrogen, oxygen, lead, chlorine and zinc in the SEM photograph in a specific embodiment of the present invention.
[0031] Figure 7g This is a diagram of the electron radiation intensity of nitrogen, oxygen, lead, chlorine and zinc in the high-zinc and low-lead alloy in a specific embodiment of the present invention.
[0032] Figure 7h This is a data diagram of the weight percentage and atomic percentage of each element on the surface of the high-zinc and low-lead alloy in a specific embodiment of the present invention. DETAILED DESCRIPTION
[0033] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work should fall within the scope of protection of the present invention.
[0034] The embodiment of the present invention intends to prepare an ammonium chloride solution by adding ammonium chloride to water, and send the lead-zinc material and the ammonium chloride solution into a leaching device for leaching to obtain a lead-zinc ammonia-chloride complex solution, and put the lead-zinc ammonia-chloride complex solution into an electrolysis device as an electrolyte for electrolysis treatment, and directly deposit it on the cathode to form a lead-zinc alloy. Since the lead-zinc ammonia-chloride complex solution is directly used for electrolysis, no complicated purification process is required, which simplifies the multi-step purification process required in the traditional electrolysis method.
[0035] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing a lead-zinc alloy using a lead-zinc ammonia-chlorine complex system. Specifically, the method for preparing a lead-zinc alloy using a lead-zinc ammonia-chlorine complex system includes, for example, the following steps:
[0036] S10: Obtaining lead-zinc-containing materials;
[0037] S20: adding ammonium chloride to water to prepare an ammonium chloride solution, and during the preparation process, no ammonia water is added and no ammonia gas is introduced;
[0038] S30: sending the lead-zinc material and the ammonium chloride solution to a leaching device for leaching to obtain a lead-zinc ammonia-chloride complex solution, and during the leaching process, no ammonia water is added and no ammonia gas is introduced;
[0039] S40: placing the lead-zinc ammonia-chlorine complex solution into an electrolytic device for electrolytic treatment to generate a lead-zinc alloy at the cathode of the electrolytic device, wherein the lead-zinc alloy is a first lead-zinc alloy, or the lead-zinc alloy includes the first lead-zinc alloy and the second lead-zinc alloy.
[0040] Specifically, in step S10, the lead-zinc-containing material is, for example, reduced volatilization fumed fly ash containing lead and zinc, and the reduced volatilization fumed fly ash containing lead and zinc is, for example, fumed fly ash obtained by reduction volatilization of smelting slag in a closed blast furnace of a lead-zinc smelter, wherein reduction fuming means that during the smelting process, the lead and zinc compounds in the lead-zinc smelting slag are reduced into lead and zinc vapor through the action of a reducing agent (such as carbon), volatilized into the upper space of the furnace and the flue system, and re-oxidized into PbO or ZnO by air or furnace gas, and captured in the dust collecting equipment to form lead-zinc fuming furnace ash.
[0041] In step S20, during the preparation of the ammonium chloride solution, no ammonia water is added and no ammonia gas is introduced, the mass of the ammonium chloride accounts for 95% of the mass of the ammonium chloride solution, and the purity of the ammonium chloride solution is industrial grade purity. The concentration of the ammonium chloride in the ammonium chloride solution is 3.0-7.0 mol / L.
[0042] In step S30, the lead-zinc smoke dust is put into the ammonium chloride solution for leaching to obtain the lead-zinc ammonia-chloride complex solution (also referred to as the lead-zinc ammonia-chloride complex leaching solution). Among them, the lead-zinc smoke dust used to prepare the lead-zinc ammonia-chloride complex solution is not limited to the fumed ash reduced by the closed blast furnace lead smelting slag, and can also be made of secondary zinc oxide ash, blast furnace gas mud, waste batteries, lead-zinc sheet scraps and other secondary lead-zinc materials, which are not specifically limited here. Zinc and lead preferentially form stable complexes with free ammonia and chloride ions in the ammonium chloride solution, ensuring that zinc and lead ions exist stably in the form of complexes during the electrolysis process, and also making it unnecessary to add additional ammonia water as an ion stabilizer to the lead-zinc ammonia-chloride complex leaching solution, avoiding the release of ammonia gas during the production process of lead-zinc alloy, thereby effectively reducing the pollution to the working environment. Among them, the composition and chemical formula of the complex may, for example, include the following categories: zinc-ammine complex, such as Zn(NH3) 2+ 、Zn(NH3)2 2+ 、Zn(NH3)3 2+ and Zn(NH3)4 2+ ; Zinc-chloride complex, such as ZnCl + 、ZnCl 2(aq) 、ZnCl3 - and ZnCl4 2- ; Lead-chlorine complex, such as PbCl + 、PbCl 2(aq) and PbCl3 - ; Zinc-ammonia-chlorine ternary complex, for example Zn(NH3)2Cl 2(aq) and Zn(NH3)2Cl3 - .
[0043] Since ammonia is irritating and corrosive, it may cause damage to human health and equipment. Compared with the traditional ammonia-ammonium salt method, ammonia will be continuously released during the production process, polluting the working environment. The preparation process in step S20 and the leaching process in step S30 of the present invention do not add ammonia water or introduce ammonia, which has significant environmental and health advantages. Specifically, the process flow of the present invention avoids the release of ammonia during the production process, thereby effectively reducing pollution to the working environment, improving the air quality in the workplace, and protecting the health of employees.
[0044] When the lead-zinc-ammonia-chlorine complex leaching solution is obtained in step S30, the ammonium chloride leaching solution may be preliminarily purified to obtain an electrolyte. For example, in the process of leaching the lead-zinc material into the ammonium chloride solution, a small amount of impurities such as iron may be leached. At this time, the lead-zinc-ammonia-chlorine complex leaching solution may be preliminarily purified to remove a small amount of impurities therein and reduce the impact on electrolysis.
[0045] In step S40, the electrolysis device includes, for example, an electrolytic cell, and the electrolytic cell is, for example, made of PVC (Polyvinylchloride) material. The PVC material has good corrosion resistance and is suitable for the construction of the electrolytic cell, which helps to improve the durability and safety of the electrolytic cell. The lead-zinc ammonia-chlorine complex leaching solution obtained in step S30 is used as an electrolyte and placed in a PVC electrolytic cell, and electrolytic treatment is performed under certain conditions to directly deposit on the cathode to form a lead-zinc alloy. Specifically, there is no need to add alkali or acid to the lead-zinc ammonia-chlorine complex leaching solution. Since the greater the applied current density or voltage, the faster the ion deposition rate, which has an adverse effect on the morphology of the product, the present invention maintains a relative stability of the ion deposition rate by controlling the conditions, which helps to improve the electrolysis efficiency and product quality.
[0046] Specifically, the lead content in the lead-zinc-ammonia-chloride complex leachate is greater than or equal to 0.1 mol / L, and the zinc content in the lead-zinc-ammonia-chloride complex leachate is greater than or equal to 0.7 mol / L. The ammonium chloride content in the lead-zinc-ammonia-chloride complex leachate is greater than or equal to 3.0 mol / L, which helps maintain the stability of the electrolyte and is conducive to maintaining the continuity of the electrolysis process.
[0047] The electrolytic cell is provided with a cathode and an anode, the anode is used for oxidation reaction in electrolysis treatment, the cathode is used for reduction reaction in electrolysis treatment, and the lead-zinc alloy is generated on the cathode. The cathode is a titanium plate, and the anode is a ruthenium-coated titanium mesh. The present invention sets the cathode as a titanium plate. Since titanium has excellent corrosion resistance, it can withstand chemical reactions in the electrolysis process, and has high electrical conductivity, which is conducive to the transmission of current. The present invention sets the ruthenium-coated titanium mesh as the anode. Since ruthenium has high electrical conductivity and high catalytic activity, it can improve the electrolysis efficiency and reduce corrosion and passivation in the anode process. In other embodiments, the anode can also be a conductive material such as a graphite plate, a titanium plate, a stainless steel plate, etc. The components of the anode are required to be free of lead and zinc, not react with the electrolyte, and its oxidation reaction potential is higher than the oxidation dissolution potential of lead and zinc, so as to prevent the anode or the lead and zinc in the anode from dissolving and contaminating the electrolyte. The cathode can also be a conductive material such as an aluminum plate and a stainless steel plate that does not react with the electrolyte.
[0048] Preferably, the distance between the cathode and the anode in the embodiment of the present invention is set to 3-5 cm. By setting a suitable pole distance, the embodiment of the present invention can prevent excessive cathode products from causing the positive and negative pole plates to be connected, thereby avoiding the formation of a short circuit.
[0049] Specifically, the electrolyte is placed in an electrolytic cell, the anode and the cathode are connected to a DC circuit, and the electrolyte is electrolyzed under high temperature conditions by controlling the electrolytic cell. The control conditions of the electrolysis treatment include electrolysis temperature and current density. The electrolysis temperature is 70 to 90° C., and the current density is 200 to 500 A / m2 The electrolytic cell is controlled to have an electrolyte temperature of 70 to 90°C and a current density of 200 to 500 A / m 2 , thus, the lead-zinc material will undergo a reduction reaction at the cathode, and the lead-zinc alloy will be generated on the cathode, and the reaction equation is:
[0050] ZnCl 2(aq) +2e=Zn+2Cl – ;
[0051] Zn(NH3)4 2+ +2e=Zn+4NH 3(aq) ;
[0052] PbCl3 – +2e=Pb+3Cl – .
[0053] The reduction reaction of the two metal ions is carried out simultaneously, and the lead-zinc alloy is obtained by synchronous precipitation. Optionally, after the lead-zinc alloy is generated in step S40, the lead-zinc alloy can be stripped and cleaned to remove the solute precipitated when the product is taken out to avoid affecting the purity of the lead-zinc alloy.
[0054] Specifically, the temperature of the electrolytic treatment is 70-90°C, and the current density of the electrolytic treatment is 200-500A / m 2 By optimizing the electrolytic treatment temperature and current density to 70-90°C and 200-500A / m 2 , which is beneficial to improve the electrolysis efficiency and product quality. When the electrolysis temperature is 70-90°C, the chemical reaction rate can be accelerated, thereby improving the overall efficiency of the electrolysis process. The increase in temperature usually increases the mobility of ions and reduces the resistance during the electrolysis process. The current density is 200-500A / m 2 It is beneficial to accelerate the reduction rate of metal ions at the cathode, that is, it is beneficial to accelerate the deposition rate.
[0055] The control conditions of the electrolytic treatment also include electrodeposition time, which includes a first electrodeposition time and a second electrodeposition time; when the electrodeposition time is the first electrodeposition time, the lead-zinc alloy is the first lead-zinc alloy; when the electrodeposition time is the second electrodeposition time, the lead-zinc alloy includes the first lead-zinc alloy and the second lead-zinc alloy.
[0056] The method for preparing lead-zinc alloy by using lead-zinc ammonia-chlorine complex system provided by the present invention can prepare lead-zinc alloy with different contents according to different electrodeposition time, and the product has wide application. If the lead content in the product is higher than the zinc content, it is a high-lead and low-zinc alloy; if the zinc content is higher than the lead content, it is a high-zinc and low-lead alloy. In actual production, the identification and discrimination of the two alloys, high-lead and low-zinc alloy and high-zinc and low-lead alloy, are determined by the product morphology and the atomic percentage content thereof. The lead-zinc material will undergo a reduction reaction at the cathode to generate a lead-zinc alloy. Specifically, the lead-zinc alloy is a first lead-zinc alloy, or the lead-zinc alloy includes the first lead-zinc alloy and the second lead-zinc alloy, the first lead-zinc alloy is a high-lead and low-zinc alloy, and the second lead-zinc alloy is a high-zinc and low-lead alloy.
[0057] When the electrodeposition time of the electrolytic treatment is less than or equal to 45 minutes, the lead-zinc alloy is the first lead-zinc alloy, that is, a high-lead, low-zinc alloy. Since the zinc ion content in the electrolyte is higher than the lead ion content, according to the electrode potential of ion discharge, lead ions are precipitated before zinc ions. On the basis of satisfying the control conditions such as electrolysis temperature and current density in the aforementioned electrolytic treatment, when the electrodeposition time of the electrolytic treatment is less than or equal to 45 minutes, the cathode product includes a high-lead, low-zinc alloy, and the high-lead, low-zinc alloy is formed at the cathode, and the high-lead, low-zinc alloy is, for example, in the shape of leaves.
[0058] When the electrodeposition time of the electrolytic treatment is greater than or equal to 45 minutes and less than or equal to 60 minutes, the lead-zinc alloy includes a first lead-zinc alloy and a second lead-zinc alloy, that is, the lead-zinc alloy includes a high-lead and low-zinc alloy and a high-zinc and low-lead alloy. On the basis of satisfying the control conditions such as the electrolytic temperature and current density in the aforementioned electrolytic treatment, the high-lead and low-zinc alloy continues to grow, and the high-zinc and low-lead alloy takes the high-lead and low-zinc alloy as a substrate, and begins to nucleate and grow, and the high-zinc and low-lead alloy is, for example, sponge-like.
[0059] When the electrodeposition time of the electrolytic treatment is greater than or equal to 60 minutes, the lead-zinc alloy includes the first lead-zinc alloy and the second lead-zinc alloy, that is, the lead-zinc alloy includes a high-lead and low-zinc alloy and a high-zinc and low-lead alloy. On the basis of satisfying the control conditions such as the electrolysis temperature and current density in the aforementioned electrolytic treatment, when the electrodeposition time of the electrolytic treatment is greater than or equal to 60 minutes, the cathode product includes a high-lead and low-zinc alloy and a high-zinc and low-lead alloy, the high-lead and low-zinc alloy no longer grows, and the high-zinc and low-lead alloy continues to nucleate and grow with the high-lead and low-zinc alloy as the substrate.
[0060] The present invention can generate alloys with different lead-zinc ratios according to the needs of specific applications by controlling the electrodeposition time of the electrolytic treatment, thereby meeting the specific requirements of different industrial fields for material properties.
[0061] Optionally, after the lead-zinc alloy is generated in step S40, the lead-zinc alloy may be stripped and cleaned to remove the solute precipitated when the product is taken out, so as to avoid affecting the purity of the lead-zinc alloy.
[0062] Furthermore, if it is necessary to prepare a sponge-like high-zinc, low-lead alloy, after the electrolysis is completed and the cathode product is stripped off, a glass blade or other suitable tool can be used to strip off the leaf-shaped high-lead, low-zinc alloy at the bottom to obtain a sponge-like high-zinc, low-lead alloy.
[0063] Optionally, during the electrolysis process, a solid lead-zinc alloy formation reaction occurs at the cathode of the system, and an ammonium ion oxidation reaction also occurs in the solution to produce gaseous nitrogen (for example, the reaction formula is: 2NH4 + –6e=N2(g)+8H + ), since the liquid used in leaching is only ammonium chloride solution, the ammonium radicals in the leaching solution are consumed after electrolysis, and thus, after collecting the lead dioxide, the waste electrolyte produced lacks ammonium radicals. At this time, ammonia water is added to the waste electrolyte. Since ammonia water, as an ammonia-containing reagent without other impurities, can effectively supplement ammonium radicals, the ammonium radicals can be effectively supplemented after ammonia water is added to the waste electrolyte. Thus, the obtained mixed solution contains sufficient ammonium radicals. This method allows the waste electrolyte to be recycled, thereby saving materials and avoiding the pollution to the environment caused by improper treatment of the waste electrolyte, thereby improving the environmental protection effect. Of course, in this embodiment, ammonium chloride can also be directly added to the waste electrolyte.
[0064] Furthermore, taking the fumed ash obtained by reducing and volatilizing the smelting slag in the closed blast furnace of the lead-zinc smelter as an example, when the slag in the closed blast furnace is fumed in the fuming furnace, dusty SO2 flue gas will also be generated. The dusty SO2 flue gas is dust-collected and purified to obtain SO2-containing flue gas. In this embodiment, the SO2-containing flue gas can be used to produce sulfuric acid. After the dust-containing SO2 flue gas is dust-collected and purified, other substances except the SO2-containing flue gas are collected to obtain fumed ash to provide the lead-zinc material. This method can make full use of the dusty SO2 flue gas generated when the slag in the closed blast furnace is fumed in the fuming furnace, thereby avoiding the pollution of the environment due to improper treatment of the SO2-containing flue gas, thereby improving the environmental protection effect.
[0065] like Figure 2 As shown, a method for preparing a lead-zinc alloy by a lead-zinc ammonia-chlorine complex system provided in an embodiment of the present invention, before the lead-zinc ammonia-chlorine complex leaching solution is placed in the electrolytic cell for the electrolytic treatment, for example, comprises the following steps:
[0066] S401: Adding an electrodeposition additive to the lead-zinc-ammonia-chlorine complex solution to obtain a lead-zinc-ammonia-chlorine complex solution after adding bone glue. For example, in this embodiment, the electrodeposition additive is bone glue. In other embodiments, the electrodeposition additive can also be other applicable additives, which are not specifically limited here. Bone glue is, for example, a protein organic substance made by hydrolyzing, extracting and drying collagen contained in animal bones, tendons or hooves.
[0067] The amount of bone glue added is 10-50 mg / L. Furthermore, the main component of bone glue is the amino acid component in collagen protein, and its molecular formula can be expressed as H2NCH2RCOOH. The amino acid component in collagen protein includes acidic amino acid glutamic acid (Glutamic acid, HOOC-(CH2) 2- ) and basic amino acids such as arginine (Arginine, HN = C (NH2) -NH- (CH2) 3- ), Lysine (Lysine, H2N-(CH2) 4- ) and the sulfur-containing amino acid methionine (Methionine, CH3-S-(CH2) 2- ) etc. Bone glue, as a commonly used electrodeposition additive, has the effects of smoothing the surface, inhibiting the side effects of impurity ions and smoothing the product morphology. In this embodiment, although the raw material reagents prepared by the electrolyte are of high purity, there are still a small amount of impurities. In this embodiment, bone glue is added to the electrolyte to make the bone glue completely dissolved in the electrolyte. Bone glue is beneficial to inhibit the influence of impurities and smooth the morphology of the electrodeposition product (in this embodiment, the product is a lead-zinc alloy). For example, the morphology of the sponge-like high-zinc and low-lead alloy is made denser, and serious shedding and dissociation phenomena are avoided during the removal of the cathode product. The present invention does not require the use of a large amount of organic reagents, reduces the dependence on other organic reagents, and reduces costs.
[0068] The present invention prepares an ammonium chloride solution by adding ammonium chloride to water, and feeds the lead-zinc material and the ammonium chloride solution into a leaching device for leaching to obtain a lead-zinc ammonia-chloride complex solution, and the lead-zinc ammonia-chloride complex leachate is placed in an electrolytic device as an electrolyte for electrolytic treatment, and is directly deposited on the cathode to form a lead-zinc alloy. Since the lead-zinc ammonia-chloride complex solution is directly used for electrolysis as an electrolyte, no complicated purification process is required, which simplifies the multi-step purification process required in the traditional electrolysis method, and in the process flow of the present invention, the ammonium chloride solution is prepared under the condition of no ammonia water and no ammonia gas, and the lead-zinc material and the ammonium chloride solution are fed into the leaching device for leaching under the condition of no ammonia water and no ammonia gas, thereby avoiding the release of ammonia gas during the production process, thereby effectively reducing the pollution to the working environment, improving the air quality in the workplace, and protecting the health of employees. The present invention can customize alloys with different lead-zinc ratios according to the needs of specific applications by controlling the electrodeposition time of the electrolytic treatment, and meet the specific requirements of different industrial fields for material properties. Specific embodiments
[0070] First, ammonium chloride is added to water to prepare 500mL of ammonium chloride solution, and no ammonia water is added or ammonia gas is introduced during the preparation process. The mass ratio of ammonium chloride to the mass ratio of ammonium chloride solution is 95%, and the concentration of ammonium chloride in the ammonium chloride solution is 7.0mol / L. The smelting slag of a closed blast furnace of a lead-zinc smelter is reduced and volatilized to smoke ash as a material containing lead and zinc, and no ammonia water is added or ammonia gas is introduced during the leaching process, and the ash is added to 500mL of ammonium chloride solution for leaching to obtain a lead-zinc ammonia-chloride complex solution (also referred to as a lead-zinc ammonia-chloride complex leachate). Wherein, the lead ion content in the lead-zinc ammonia-chloride complex leachate is about 21g / L, and the zinc ion content is about 56g / L. Then, bone glue was added to the lead-zinc ammonia-chlorine complex leaching solution at a dosage of 10-50 mg / L, and then the anode ruthenium-coated titanium mesh and the cathode titanium plate were connected to the DC circuit. The distance between the anode and the cathode was controlled at 4 cm. The electrolyte temperature was maintained at 80 ° C and the current density was 400 A / m by controlling the electrolytic cell. 2 , so that lead-zinc alloy can be produced at the cathode.
[0071] When the electrodeposition time of the electrolytic treatment is controlled to be 30 min, a high-lead and low-zinc alloy can be prepared on the cathode plate. The macroscopic morphology of the high-lead and low-zinc alloy prepared on the cathode plate is shown in FIG. Figure 3 As shown in Figure 2, the morphology of high-lead and low-zinc alloys presents a leaf-like distribution. Figure 6a~6h , Figure 6a This is a scanning electron microscope (SEM) image of the morphology of a high-lead, low-zinc alloy. Figure 6b to Figure 6f 6a is the element distribution area diagram of nitrogen, oxygen, lead, chlorine and zinc in the high-lead and low-zinc alloy in this embodiment. Figure 6d The distribution range of metal lead is the central trunk of the leaf-shaped product. Figure 6f , while the distribution of metallic zinc is in the edge area of the leaf-shaped products. Figure 6a~6f As shown in the figure, the morphology of the high-lead and low-zinc alloys shows a leaf-like distribution, which is consistent with Figure 3 The macroscopic results shown are consistent. Figure 6g : is a graph of the electron radiation intensity of nitrogen, oxygen, lead, chlorine and zinc in the high-lead and low-zinc alloy in a specific embodiment of the present invention, from Figure 6g The height of the displayed electron intensity peak can tell the main elements of the product, and then determine that the product is a high-lead, low-zinc alloy. Figure 6h The weight percentage and atomic percentage data of nitrogen, oxygen, lead, chlorine and zinc in the high-lead and low-zinc alloy in the specific embodiment of the present invention are shown in FIG. Figure 6h The specific content of lead and zinc elements in the generated high-lead and low-zinc alloy can be known. Figure 6h is based on Figure 6b to Figure 6g The element distribution area diagram of nitrogen, oxygen, lead, chlorine and zinc, the weight percentage and atomic percentage data of each element in the high-lead and low-zinc alloy calculated from the electron radiation intensity, etc.
[0072] When the electrodeposition time of the electrolytic treatment is controlled to be 2 h, a high-zinc and low-lead alloy can be prepared at the cathode plate. The macroscopic morphology of the high-zinc and low-lead alloy prepared at the cathode plate is shown in FIG. Figure 4 As shown in Figure 2, the overall morphology of the high zinc and low lead alloy is sponge-like. Figures 7a to 7h , Figure 7a This is a scanning electron microscope (SEM) image of the morphology of high zinc and low lead alloy. Figure 7b to Figure 7f 7a is the element distribution area diagram of nitrogen, oxygen, lead, chlorine and zinc in the high zinc and low lead alloy in this embodiment. Figure 7d The distribution range of metal lead is the central trunk of the leaf-shaped product. Figure 7f , while the distribution of metallic zinc is in the edge area of the leaf-shaped products. Figures 7a to 7f As shown in the figure, the sponge-like high-zinc and low-lead alloy is actually composed of many tiny needle-shaped or rod-shaped alloys, which is consistent with Figure 4 The macroscopic results shown are consistent. Figure 7g : is a graph of the electron radiation intensity of nitrogen, oxygen, lead, chlorine and zinc in the high-zinc and low-lead alloy in a specific embodiment of the present invention, from Figure 7g The height of the displayed electron intensity peak can tell the main elements of the product, and then determine that the product is a high-zinc, low-lead alloy. Figure 7h The weight percentage and atomic percentage data of nitrogen, oxygen, lead, chlorine and zinc in the high-zinc and low-lead alloy in the specific embodiment of the present invention are shown in FIG. Figure 7h The specific content of lead and zinc elements in the generated high-zinc and low-lead alloy can be known. Figure 7h is based on Figure 7b to Figure 7g The element distribution area diagram of nitrogen, oxygen, lead, chlorine and zinc, the weight percentage and atomic percentage data of each element in the high-zinc and low-lead alloy calculated from the electron radiation intensity, etc.
[0073] Reference Figure 5 , Figure 5 The graph of the cathode metal recovery rate of the electrolytic cell versus electrolysis time in a specific embodiment of the present invention is as follows: Figure 5 The recovery rate of lead and zinc metals in the electrolyte after 2.0h of continuous electrolysis without product stripping. Figure 5 It can be seen that the current density of the electrolytic treatment is 300A / m 2 When the lead and zinc recovery rates are low, that is, the amount of lead-zinc alloy deposition is low, and the current density of the electrolytic treatment is 500A / m 2 When the lead and zinc recovery rates are high, that is, the amount of lead-zinc alloy deposited is large, indicating that a faster current density is conducive to accelerating the reduction rate of metal ions on the cathode, that is, it is conducive to accelerating the deposition rate. Figure 5 It can also be seen that when the electrodeposition time of the electrolytic treatment does not exceed 45 minutes, the ratio of lead to zinc in the lead-zinc alloy generated at the cathode is relatively large, and the lead-zinc alloy at this stage is a high-lead and low-zinc alloy; when the electrodeposition time of the electrolytic treatment exceeds 60 minutes, the ratio of lead to zinc in the lead-zinc alloy generated at the cathode is relatively small, and the lead-zinc alloy at this stage is a high-zinc and low-lead alloy. The high-zinc and low-lead alloy will form and grow on the surface of the high-lead and low-zinc alloy in a short time.
[0074] Among them, the recovery rate of lead and zinc metal is obtained by removing part of the electrolyte and using EDTA titration (i.e., ethylenediaminetetraacetic acid titration, which is a commonly used analytical chemistry method, using ethylenediaminetetraacetic acid as a titrant to determine the content of metal ions). In this embodiment, according to the electrolysis rate obtained by titration and the actual experimental effect, the electrolysis time does not exceed 45min, and the products at the cathode plate are all high-lead and low-zinc alloys; when the electrolysis time is 45-60min, the high-zinc and low-lead alloys are nucleated and grown with the high-lead and low-zinc alloys as the substrate, and there are both high-lead and low-zinc and high-zinc and low-lead alloys in this time period; the electrolysis time exceeds 60min, and the products are all high-zinc and low-lead alloys, that is, the high-zinc and low-lead alloys continue to grow, while the high-lead and low-zinc alloys no longer grow. The present invention can generate alloys with different lead-zinc ratios according to the needs of specific applications by controlling the electrodeposition time of the electrolytic treatment, meeting the specific requirements of different industrial fields for material properties.
[0075] Optionally, after the lead-zinc alloy is generated by electrolysis, the lead-zinc alloy can be stripped and cleaned to remove the solute precipitated when the product is taken out, so as to avoid affecting the purity of the lead-zinc alloy.
[0076] Furthermore, if it is necessary to prepare a sponge-like high-zinc, low-lead alloy, after the electrolysis is completed and the cathode product is stripped off, a glass blade or other suitable tool can be used to strip off the leaf-shaped high-lead, low-zinc alloy at the bottom to obtain a sponge-like high-zinc, low-lead alloy.
[0077] The embodiment of the present invention prepares an ammonium chloride solution by adding ammonium chloride to water, and feeds the lead-zinc material and the ammonium chloride solution into a leaching device for leaching to obtain a lead-zinc ammonia-chloride complex solution, and the lead-zinc ammonia-chloride complex leachate is placed in an electrolytic device as an electrolyte for electrolytic treatment, and is directly deposited on the cathode to form a lead-zinc alloy. Since the lead-zinc ammonia-chloride complex solution is directly used for electrolysis, no complicated purification process is required, which simplifies the multi-step purification process required in the traditional electrolysis method, and the method has the advantages of simple and controllable operation, low cost and environmental friendliness. In the process flow of the present invention, the ammonium chloride solution is prepared under the condition of no ammonia water and no ammonia gas, and the lead-zinc material and the ammonium chloride solution are fed into the leaching device for leaching under the condition of no ammonia water and no ammonia gas, thereby avoiding the release of ammonia gas during the production process, thereby effectively reducing the pollution to the working environment, improving the air quality in the workplace, and protecting the health of employees.
[0078] The above is a description of the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which will not affect the essence of the present invention.
[0079] In addition, it can be understood that the aforementioned embodiments are only exemplary descriptions of the present invention. Under the premise that the technical features do not conflict, the structures do not contradict, and the purpose of the present invention is not violated, the technical solutions of the various embodiments can be arbitrarily combined and used in combination.
[0080] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a lead-zinc alloy using a lead-zinc ammonia-chlorine complex system, characterized in that: include: Obtaining lead-zinc containing materials; Adding ammonium chloride to water to prepare an ammonium chloride solution, and during the preparation process, no ammonia water is added and no ammonia gas is introduced; The lead-zinc material and the ammonium chloride solution are sent to a leaching device for leaching to obtain a lead-zinc ammonia-chloride complex solution, and no ammonia water is added and no ammonia gas is introduced during the leaching process; The lead-zinc ammonia-chlorine complex solution is placed in an electrolytic device for electrolytic treatment to generate a lead-zinc alloy at the cathode of the electrolytic device. The lead-zinc alloy is a first lead-zinc alloy, or the lead-zinc alloy includes the first lead-zinc alloy and the second lead-zinc alloy.
2. The method for preparing lead-zinc alloy by using a lead-zinc-ammonia-chlorine complex system according to claim 1, characterized in that: The lead content in the lead-zinc-ammonia-chloride complex solution is greater than or equal to 0.1 mol / L, the zinc content in the lead-zinc-ammonia-chloride complex solution is greater than or equal to 0.7 mol / L, and the ammonium chloride content in the lead-zinc-ammonia-chloride complex solution is greater than or equal to 3.0 mol / L.
3. The method for preparing lead-zinc alloy by using lead-zinc ammonia-chlorine complex system according to claim 2, characterized in that: The control conditions of the electrolysis treatment include electrolysis temperature and current density. The electrolysis temperature is 70-90°C, and the current density is 200-500A / m 2 .
4. The method for preparing lead-zinc alloy by using lead-zinc ammonia-chlorine complex system according to claim 3, characterized in that: The control conditions of the electrolytic treatment also include electrodeposition time, which includes a first electrodeposition time and a second electrodeposition time; when the electrodeposition time is the first electrodeposition time, the lead-zinc alloy is the first lead-zinc alloy; when the electrodeposition time is the second electrodeposition time, the lead-zinc alloy includes the first lead-zinc alloy and the second lead-zinc alloy.
5. The method for preparing lead-zinc alloy by using lead-zinc ammonia-chlorine complex system according to claim 4, characterized in that: The first electrodeposition time is less than or equal to 45 minutes; the second electrodeposition time is greater than or equal to 60 minutes.
6. The method for preparing lead-zinc alloy by using a lead-zinc-ammonia-chlorine complex system as claimed in claim 5, characterized in that: The first lead-zinc alloy is a high-lead and low-zinc alloy, and the second lead-zinc alloy is a high-zinc and low-lead alloy.
7. The method for preparing lead-zinc alloy by using lead-zinc ammonia-chlorine complex system according to claim 4, characterized in that: The electrolysis device comprises an electrolytic cell, the electrolytic cell is provided with the cathode and the anode, and the electrolytic cell is a polyvinyl chloride electrolytic cell.
8. The method for preparing lead-zinc alloy by using lead-zinc ammonia-chlorine complex system according to claim 7, characterized in that: The cathode is a titanium plate, and the anode is a ruthenium-coated titanium mesh.
9. The method for preparing lead-zinc alloy by using lead-zinc ammonia-chlorine complex system according to claim 1, characterized in that: Before the lead-zinc-ammonia-chlorine complex solution is placed in the electrolytic cell for the electrolytic treatment, the method comprises: The electrodeposition additive is added to the lead-zinc-ammonia-chlorine complex solution to obtain the lead-zinc-ammonia-chlorine complex solution after the electrodeposition additive is added.
10. The method for preparing lead-zinc alloy by using lead-zinc-ammonia-chlorine complex system according to claim 9, characterized in that: The electrodeposition additive is bone glue, and the dosage of the electrodeposition additive is 10-50 mg / L.