Method for preparing high-modulus para-aramid fiber by using superheated steam
Through two-stage heat treatment of para-aramid wet fibers, superheated steam is used to remove moisture from the fibers and establish more hydrogen bonds, which solves the problems of insufficient room for modulus improvement of para-aramid fibers and production safety risks in the prior art. It realizes efficient and low-cost high-modulus para-aramid fiber preparation, which is suitable for large-scale production line applications.
Patent Information
- Application Number
- CN202411398814.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-10-08
AI Technical Summary
In the prior art, the preparation process of para-aramid has high temperature and high pressure state, which has production safety risks, high equipment requirements, large production costs, complex process flow, and difficult to achieve large-scale production line application. The multi-stage stretching treatment time is long and wastewater recycling is used. Difficulty, failure to effectively improve the high modulus performance of the fiber.
The para-aramid wet fiber obtained by dry spraying method is subjected to two-stage heat treatment, and superheated steam at 200-350°C is used to perform heat treatment. The temperature fluctuations in the heat box are reduced by primary and secondary heat treatment respectively, and superheated steam is used to perform heat treatment. High heat transfer coefficient and high permeability rapidly evaporate moisture in the fiber, promoting the establishment of hydrogen bonds between molecular chains, thereby improving the tensile modulus of the fiber.
The tensile modulus of para-aramid fiber has been increased by 10 to 20.5%, simplified the process flow, reduced energy and production costs, avoided the damage of high temperature to the fiber, comply with the principle of green production, and realized the recycling of waste gas energy. use.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer material processing and relates to a method for preparing high modulus para-aramid fiber by using superheated steam. Background Art
[0002] Aramid fiber refers to a macromolecular polymer whose main chain is composed of benzene rings and amide bonds, and at least 85% of the amide groups are directly connected to the benzene rings. Among them, para-aramid (such as PPTA, poly(p-phenylene terephthalamide)) is polymerized by p-phenylenediamine and terephthaloyl chloride, and the two amide bonds connecting the benzene rings are in the para position. The low-temperature polycondensation method is currently the most mature process for synthesizing aramid fibers. Low-temperature polycondensation usually controls the polymerization temperature at -5 to 0°C, and its purpose is to slow down the precipitation and increase the molecular weight of the macromolecular chain. At the same time, in order to prevent terephthaloyl chloride from reacting with water and water vapor to form an inhibitor, a slightly excessive amount of terephthaloyl chloride is added during polymerization to ensure the smooth progress of the polymerization reaction. The prepared PPTA polymer is dissolved in fuming sulfuric acid to form a nematic liquid crystal solution, which is then spun by dry-jet wet spinning, and becomes a finished fiber through processes such as alkali washing, water washing, drying, and winding. Para-aramid is a typical high-performance fiber with high strength, high modulus and high temperature resistance. It is often used as the reinforcing phase of materials and is widely used in safety protection, automotive industry, optical cable protection and other fields. Its position in aerospace, new energy development and other fields is irreplaceable.
[0003] In order to further improve the performance of para-aramid, Chinese patent CN102797061B provides "a multi-stage stretching process for manufacturing aramid III", which passes the aramid III fiber into two coagulation baths for negative stretching and plasticizing stretching treatment, and then washes it and enters the wet heat stretching bath again for a second plasticizing stretching treatment. The high-strength and high-modulus aramid III fiber prepared by this method has a 6.67% increase in tensile strength and a 11.76% increase in tensile modulus. However, the nascent aramid III fiber needs to undergo multiple stretching treatments, which takes a long time, and the subsequent recovery of industrial wastewater generated by multiple coagulation baths is difficult and cannot be recycled, which does not conform to the principles of green economy.
[0004] Chinese patent CN107503121B provides a "supercritical CO2 modification method and device for aramid fiber under tension in motion". This method designs a fiber tension device placed in a closed container of supercritical carbon dioxide, and winds the aramid fiber around the motion device to apply a tension of 4 to 50 cN; the carbon dioxide is placed in a supercritical state at 50 to 250 ° C and a pressure of 8 to 16 MPa, carrying isocyanate compounds or terephthaloyl chloride as a cross-linking agent; after swelling for 20 to 120 minutes, the pressure is released, the fiber is taken out, cleaned, and dried to obtain high-performance fibers. This method uses a variety of aramid fibers for impregnation and swelling, in which the elastic modulus of para-aramid is increased by 2.5 to 8.24%, and the tensile strength is increased by 8.07 to 8.65%. However, the equipment requirements are high, the production cost is high, the process flow is complicated, and there are production safety risks in the high temperature and high pressure state, which is not suitable for large-scale production lines.
[0005] Therefore, it is of great significance to study a method for preparing high modulus para-aramid using superheated steam to solve the problems existing in the prior art. Summary of the invention
[0006] The purpose of the present invention is to solve the problems existing in the prior art and provide a method for preparing high modulus para-aramid fiber by using superheated steam.
[0007] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing high modulus para-aramid fiber using superheated steam, wherein the para-aramid wet fiber obtained by dry-jet wet spinning is subjected to two-stage heat treatment in sequence to obtain the high modulus para-aramid fiber;
[0009] The first-stage heat treatment refers to heat treatment of the wet para-aramid fiber in a heat box, the temperature of the heat box is set at 200-250°C, and the heat box is passed through with a stable superheated steam at a temperature of 250-300°C;
[0010] Secondary heat treatment refers to heat treatment of the fiber after primary heat treatment in a heat box, the temperature of the heat box is set at 300-350°C, and the heat box is passed through with superheated steam at a stable temperature of 300-350°C;
[0011] The fibers entering the primary heat treatment are cold fibers, while the fibers entering the secondary heat treatment are preheated fibers. The settings of the heat box temperature and the superheated steam temperature during the two-stage heat treatment process in the present invention are to minimize the fluctuation of the actual temperature in the heat box. The above ranges are determined by the inventors after many experiments.
[0012] Compared with the control sample, the tensile modulus of the high modulus para-aramid fiber is increased by 10-20.5%; the preparation of the control sample is also to perform two-stage heat treatment on the para-aramid wet fiber obtained by dry-jet wet spinning in sequence, the only difference is that hot steam is not passed through the heat box.
[0013] In the present invention, superheated steam is used to replace the traditional protective atmosphere, and the high enthalpy value of superheated steam is used to quickly heat the moisture in the fiber to the boiling point so that it evaporates and leaves the fiber. The modulus of the high modulus para-aramid fiber in the prior art has a lot of room for improvement compared with its theoretical modulus. The main reason is that water molecules occupy the internal space of the fiber, which makes it impossible for the molecular chain segments here to form hydrogen bonds, thus forming defects. The superheated steam used in the present invention has a high heat transfer coefficient and no mass transfer resistance. It can instantly vaporize the moisture in the fiber. At this time, the fiber is in a tensioned state, and the macromolecular chain activity of the fiber is intensified under the action of high temperature and tension, and the fiber approaches each other to quickly establish more and stronger hydrogen bonds. Compared with the traditional multi-stage heat treatment used in the prior art to prepare high modulus para-aramid, the present invention only needs two-stage heat treatment to achieve a greater modulus improvement effect, and can save a lot of energy and production costs when applied to large-scale production lines.
[0014] The prior art is to prepare para-aramid wet fiber by dry-jet wet spinning, and the specific steps are as follows:
[0015] (1) Low-temperature polycondensation: Add an N-methylpyrrolidone solution containing anhydrous LiCl and pyridine to a polymerization reactor equipped with a stainless steel stirrer and passed with dry N2. Add powdered p-phenylenediamine at room temperature, cool to -5 to 0°C, and then add a slightly excess of powdered terephthaloyl chloride, the molar ratio of terephthaloyl chloride to p-phenylenediamine being 1.001 to 1.002:1. Increase the stirring speed until the yellow gel mass is crushed and let it stand for more than 6 hours. Add a small amount of water to the resulting polymer, crush it and filter it, add 8 to 15% NaOH to the mixture until the washing liquid is neutral, and then wash with water several times to remove residual solvents, impurities such as LiCl, pyridine and HCl. Dry the polymer at 100°C to obtain a dry PPTA polymer;
[0016] (2) Preparation of spinning solution: PPTA polymer and concentrated sulfuric acid are mixed to prepare a spinning solution with a PPTA mass fraction of 19 to 19.5%, and the mixture is stirred and heated to 75° C. to obtain a uniform nematic liquid crystal solution;
[0017] (3) Dry-jet wet spinning: The spinning solution is extruded from the spinneret through a metering pump, passes through an air layer of 2 to 7 mm, and has a draft ratio of 4 to 10. It then enters a coagulation bath with a temperature of 0 to 5°C and a sulfuric acid concentration of 0 to 10%. The solution is coagulated into filaments. The filaments are then washed with water and neutralized to neutrality by adding Ca(OH)2, followed by multiple washings and preliminary drying to obtain wet fibers.
[0018] As the preferred technical solution:
[0019] In the above-mentioned method for preparing high modulus para-aramid fiber using superheated steam, the moisture content of the para-aramid wet fiber obtained by dry-jet wet spinning (the percentage of the mass of water contained in the para-aramid wet fiber to the total mass of the para-aramid wet fiber) is 25-35%.
[0020] In the method for preparing high modulus para-aramid fiber using superheated steam as described above, the tension during the primary heat treatment is controlled within the range of 0.5 to 1 cN / dtex, and the tension during the secondary heat treatment is controlled within the range of 2 to 3 cN / dtex.
[0021] In the method for preparing high modulus para-aramid fiber using superheated steam as described above, the residence time of the wet para-aramid fiber in the heat box during the primary heat treatment is 2 to 3 seconds, and the moisture content of the fiber after the primary heat treatment is 10 to 15%.
[0022] In the method for preparing high modulus para-aramid fiber using superheated steam as described above, the residence time of the fiber in the heat box during the secondary heat treatment is 1 to 2 seconds, and the moisture content of the fiber after the two-stage heat treatment is 3 to 5%. A small amount of residual moisture is beneficial to the mechanical properties of the fiber.
[0023] Beneficial effects:
[0024] (1) The present invention provides a method for preparing high modulus para-aramid fiber using superheated steam, wherein superheated steam is used to replace the traditional protective atmosphere, and the unsaturated, high permeability and high thermal conductivity of the superheated steam are used to quickly remove the water molecules inside the fiber, thereby improving the fiber crystallinity and the orderliness of the fiber amorphous phase, and re-establishing more and stronger hydrogen bonds between molecular chains, thereby obtaining a para-aramid fiber with a higher modulus with minimal strength loss; and a high-efficiency, high-quality high modulus para-aramid fiber production line is established through two-stage superheated steam heat treatment, and the tensile modulus is increased by 10 to 20.5% compared with the traditional heat treatment;
[0025] (2) The present invention replaces the protective atmosphere in traditional heat treatment with superheated steam drying, avoiding the heat loss transferred from the equipment to the inert gas and prolonging the drying time. It not only greatly reduces the cost but also reduces the damage to the fiber caused by high temperature. Compared with the traditional para-aramid drying method, it can reduce the loss of fiber mechanical properties to a greater extent, that is, obtain para-aramid fiber with higher modulus with minimal strength loss. Compared with the traditional heat treatment process, the superheated steam in the present invention has stronger penetration, and its diffusion has almost no mass transfer interface resistance between different molecules. It can remove moisture from the inside of the fiber to a greater extent, thereby establishing hydrogen bonds between macromolecular chains. Compared with the para-aramid prepared by traditional multi-stage drying technology, the high modulus para-aramid obtained by this method is of higher quality;
[0026] (3) The method of preparing high modulus para-aramid fiber using superheated steam of the present invention adopts a method combining heat treatment with superheated steam drying technology, which can reduce the content of solution and water in the fiber in a short time, greatly shorten the heat treatment time and improve the efficiency of heat treatment, and solve the problems of high temperature damage, long treatment time, frequent fiber breakage and the like in the traditional high modulus para-aramid fiber preparation process; at the same time, the fiber fineness is greatly reduced and the fiber modulus is increased, so that the high modulus para-aramid fiber can be produced simply, efficiently and stably, and the production cost is reduced;
[0027] (4) The present invention does not use any chemical reagents or toxic gases, and does not emit substances harmful to the environment during the production process, which complies with the principle of green production; and superheated steam can realize waste gas energy recovery and utilization to improve energy utilization, achieve energy conservation and emission reduction, and reduce investment costs. DETAILED DESCRIPTION
[0028] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0029] The test methods involved in the performance indicators in the embodiments and comparative examples of the present invention are as follows:
[0030] Tensile modulus and strength: XQ-1 fiber tensile tester was used to test the mechanical properties of PPTA monofilament in accordance with GB / T 14337-2008. The fiber clamping distance was 20 mm, the descent rate was 10 mm / min, the modulus elongation range was 0.1% to 2%, and each group was tested 30 times to take the average value.
[0031] Example 1
[0032] A method for preparing high modulus para-aramid fiber using superheated steam, the specific steps are as follows:
[0033] (1) Para-aramid wet fibers (Sinochem High Performance Fiber Co., Ltd.) with a moisture content of 30.34% obtained by dry-jet wet spinning were subjected to primary heat treatment in a hot box, the temperature of the hot box was set at 200° C., the tension was controlled at 0.5 cN / dtex, and a stable superheated steam at a temperature of 250° C. was passed through the hot box;
[0034] Among them, the residence time of the wet para-aramid fiber in the heat box is 2 seconds, and the moisture content of the fiber after the first-level heat treatment is 14.8%;
[0035] (2) subjecting the fibers after the primary heat treatment to a secondary heat treatment in a hot box, wherein the temperature of the hot box is set at 300° C., the tension is controlled at 2 cN / dtex, and a stable superheated steam at a temperature of 300° C. is passed through the hot box to obtain a high modulus para-aramid fiber;
[0036] The residence time of the fiber in the heat box during the secondary heat treatment is 2 seconds, and the moisture content of the fiber after the two-stage heat treatment is 4.6%.
[0037] The tensile modulus of the high modulus para-aramid fiber finally obtained is 837.43 cN / dtex, which is 10.12% higher than that of the control sample; the tensile strength of the high modulus para-aramid fiber is 21.68 cN / dtex; the preparation of the control sample is basically the same as that of Example 1, and the para-aramid wet fiber obtained by dry-jet wet spinning is subjected to two-stage heat treatment in sequence, the only difference being that hot steam is not passed through the heat box.
[0038] Example 2
[0039] A method for preparing high modulus para-aramid fiber using superheated steam, the specific steps are as follows:
[0040] (1) Para-aramid wet fibers (Sinochem High Performance Fiber Co., Ltd.) with a moisture content of 30.34% obtained by dry-jet wet spinning were subjected to primary heat treatment in a hot box, the temperature of the hot box was set at 250° C., the tension was controlled at 0.5 cN / dtex, and a stable superheated steam at a temperature of 300° C. was passed through the hot box;
[0041] Among them, the residence time of the wet para-aramid fiber in the heat box is 2 seconds, and the moisture content of the fiber after the first-level heat treatment is 10.4%;
[0042] (2) subjecting the fibers after the primary heat treatment to a secondary heat treatment in a hot box, wherein the temperature of the hot box is set at 350° C., the tension is controlled at 3 cN / dtex, and a stable superheated steam at a temperature of 350° C. is passed through the hot box to obtain a high modulus para-aramid fiber;
[0043] The residence time of the fiber in the heat box during the secondary heat treatment is 1 second, and the moisture content of the fiber after the two-stage heat treatment is 3.5%.
[0044] The tensile modulus of the high modulus para-aramid fiber finally obtained is 895.45 cN / dtex, which is 17.75% higher than that of the control sample; the tensile strength of the high modulus para-aramid fiber is 20.73 cN / dtex; the preparation of the control sample is basically the same as that of Example 2, and the para-aramid wet fiber obtained by dry-jet wet spinning is subjected to two-stage heat treatment in sequence, the only difference being that hot steam is not passed through the heat box.
[0045] Example 3
[0046] A method for preparing high modulus para-aramid fiber using superheated steam, the specific steps are as follows:
[0047] (1) Para-aramid wet fibers (Sinochem High Performance Fiber Co., Ltd.) with a moisture content of 30.34% obtained by dry-jet wet spinning were subjected to primary heat treatment in a hot box, the temperature of the hot box was set at 250° C., the tension was controlled at 1 cN / dtex, and a stable superheated steam at a temperature of 300° C. was passed through the hot box;
[0048] Among them, the residence time of the para-aramid wet fiber in the heat box is 3 seconds, and the moisture content of the fiber after the first-level heat treatment is 10.1%;
[0049] (2) subjecting the fibers after the primary heat treatment to a secondary heat treatment in a hot box, wherein the temperature of the hot box is set at 350° C., the tension is controlled at 2 cN / dtex, and a stable superheated steam at a temperature of 350° C. is passed through the hot box to obtain a high modulus para-aramid fiber;
[0050] The residence time of the fiber in the heat box during the secondary heat treatment is 2 seconds, and the moisture content of the fiber after the two-stage heat treatment is 3.1%.
[0051] The tensile modulus of the high modulus para-aramid fiber finally obtained is 862.53 cN / dtex, which is 13.42% higher than that of the control sample; the tensile strength of the high modulus para-aramid fiber is 20.13 cN / dtex; the preparation of the control sample is basically the same as that of Example 3, and the para-aramid wet fiber obtained by dry-jet wet spinning is subjected to two-stage heat treatment in sequence, the only difference being that hot steam is not passed through the heat box.
[0052] Example 4
[0053] A method for preparing high modulus para-aramid fiber using superheated steam, the specific steps are as follows:
[0054] (1) Para-aramid wet fibers (Sinochem High Performance Fiber Co., Ltd.) with a moisture content of 30.34% obtained by wet spinning were subjected to primary heat treatment in a hot box, the temperature of the hot box was set at 250° C., the tension was controlled at 1 cN / dtex, and a stable superheated steam at a temperature of 300° C. was passed through the hot box;
[0055] Among them, the residence time of the wet para-aramid fiber in the heat box is 3 seconds, and the moisture content of the fiber after the first-level heat treatment is 10.1%;
[0056] (2) subjecting the fibers after the primary heat treatment to a secondary heat treatment in a hot box, wherein the temperature of the hot box is set at 300° C., the tension is controlled at 2 cN / dtex, and a stable superheated steam at a temperature of 350° C. is passed through the hot box to obtain a high modulus para-aramid fiber;
[0057] The residence time of the fiber in the heat box during the secondary heat treatment is 1 second, and the moisture content of the fiber after the two-stage heat treatment is 3.3%.
[0058] The tensile modulus of the high modulus para-aramid fiber finally obtained is 889.21 cN / dtex, which is 16.93% higher than that of the control sample; the tensile strength of the high modulus para-aramid fiber is 20.56 cN / dtex; the preparation of the control sample is basically the same as that of Example 4, and the para-aramid wet fiber obtained by dry-jet wet spinning is subjected to two-stage heat treatment in sequence, the only difference being that hot steam is not passed through the heat box.
[0059] Example 5
[0060] A method for preparing high modulus para-aramid fiber using superheated steam, the specific steps are as follows:
[0061] (1) para-aramid wet fibers (Sinochem High Performance Fiber Co., Ltd.) with a moisture content of 30.34% obtained by dry-jet wet spinning were subjected to primary heat treatment in a hot box, the temperature of the hot box was set at 225° C., the tension was controlled at 0.75 cN / dtex, and a stable superheated steam at a temperature of 275° C. was passed through the hot box;
[0062] Among them, the residence time of the wet para-aramid fiber in the heat box is 3 seconds, and the moisture content of the fiber after the first-level heat treatment is 10.3%;
[0063] (2) subjecting the fibers after the primary heat treatment to a secondary heat treatment in a hot box, wherein the temperature of the hot box is set at 325° C., the tension is controlled at 2.5 cN / dtex, and a stable superheated steam at a temperature of 325° C. is passed through the hot box to obtain a high modulus para-aramid fiber;
[0064] The residence time of the fiber in the heat box during the secondary heat treatment is 2 seconds, and the moisture content of the fiber after the two-stage heat treatment is 3.4%.
[0065] The tensile modulus of the high modulus para-aramid fiber finally obtained is 916.37 cN / dtex, which is 20.5% higher than that of the control sample; the tensile strength of the high modulus para-aramid fiber is 20.64 cN / dtex; the preparation of the control sample is basically the same as that of Example 5, and the para-aramid wet fiber obtained by dry-jet wet spinning is subjected to two-stage heat treatment in sequence, the only difference being that hot steam is not passed through the heat box.
Claims
1. A method for preparing high modulus para-aramid fiber using superheated steam, characterized in that: The p-aramid wet fiber obtained by dry-jet wet spinning is subjected to two-stage heat treatment in sequence to obtain high modulus p-aramid; The first-stage heat treatment refers to heat treatment of the wet para-aramid fiber in a heat box, the temperature of the heat box is set at 200-250°C, and the heat box is passed through with a stable superheated steam at a temperature of 250-300°C; Secondary heat treatment refers to heat treatment of the fiber after primary heat treatment in a heat box, the temperature of the heat box is set at 300-350°C, and the heat box is passed through with a stable superheated steam at a temperature of 300-350°C; Compared with the control sample, the tensile modulus of the high modulus para-aramid fiber is increased by 10-20.5%; the preparation of the control sample is also to perform two-stage heat treatment on the para-aramid wet fiber obtained by dry-jet wet spinning in sequence, the only difference is that hot steam is not passed through the heat box.
2. The method for preparing high modulus para-aramid fiber using superheated steam according to claim 1, characterized in that: The moisture content of the para-aramid wet fiber obtained by dry-jet wet spinning is 25-35%.
3. The method for preparing high modulus para-aramid fiber using superheated steam according to claim 1, characterized in that: The tension during the primary heat treatment is controlled within the range of 0.5 to 1 cN / dtex, and the tension during the secondary heat treatment is controlled within the range of 2 to 3 cN / dtex.
4. The method for preparing high modulus para-aramid fiber using superheated steam according to claim 1, characterized in that: During the primary heat treatment, the residence time of the wet para-aramid fiber in the heat box is 2 to 3 seconds, and the moisture content of the fiber after the primary heat treatment is 10 to 15%.
5. The method for preparing high modulus para-aramid fiber using superheated steam according to claim 1, characterized in that: During the secondary heat treatment, the residence time of the fiber in the heat box is 1 to 2 seconds, and the moisture content of the fiber after the two-stage heat treatment is 3 to 5%.
Citation Information
Patent Citations
Continuously static spinning method of polyamide 6 / 66 copolymer filament yarn
CN101037809A
Producing high molecular weight polyamide from nitrile
CN1136572A
On-line fiber heat treatment
US5174046A
Cellulose fiber continuous preparation method
WO2021135705A1
AU6451580A
Cited By
Method for preparing high-modulus para-aramid fiber by using benzoxazine coating containing functional particles
CN121110372A