Temperature response type composite fiber material and preparation method thereof
By using composite fiber materials of PNIPAM, graphene and PCM, the shortcomings of existing temperature-responsive materials in terms of flexibility, response speed, energy consumption and stability are overcome, achieving rapid response, efficient thermal conduction and precise temperature regulation, and providing excellent cycle stability and adaptive thermal management.
Patent Information
- Application Number
- CN202411139041.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
Existing temperature-responsive materials lack flexibility in dealing with complex and variable environmental temperatures, making it difficult to achieve rapid response, efficient heat conduction, precise temperature regulation, and good cycle stability. Furthermore, traditional materials suffer from problems such as high energy consumption, slow response speed, and poor cycle stability.
By employing composite fiber materials of poly(N-isopropylacrylamide) (PNIPAM), graphene, and phase change material (PCM), and through careful design of component ratios and preparation processes, a synergistic effect of multiple thermal management mechanisms is achieved, including the temperature sensitivity of PNIPAM, the efficient thermal conductivity network of graphene, and the phase change regulation of PCM.
It achieves rapid response to temperature changes, adaptive thermal conductivity, precise temperature control, and excellent cycling stability, possesses efficient thermal comfort adjustment capabilities, and maintains good mechanical and processing properties.
Smart Images

Figure BDA0005000223840000151 
Figure BDA0005000223840000161 
Figure BDA0005000223840000162
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite fiber materials, in particular to a temperature-responsive composite fiber material and a preparation method thereof. Background Art
[0002] In recent years, with the growing demand for personal thermal management, the research and development of smart temperature-regulating textiles has received widespread attention. Traditional temperature-regulating materials usually rely on a single thermal management mechanism, such as thermal conductive materials reported by Li et al. in Advanced Materials (2023, Vol. 35, pp. 2209825), or phase change materials introduced by Zhang et al. in Advanced Science (2023, Vol. 10, pp. 2305228). However, these single-mechanism materials are often not flexible enough to cope with complex and changing ambient temperatures.
[0003] In addition, existing temperature-responsive materials also have some limitations. For example, the electrothermal textiles described by Repon et al. in the journal Materials (2021, Vol. 14, p. 6540) can actively generate heat, but have high energy consumption and difficulty in achieving precise temperature control. Temperature-responsive materials based on shape memory polymers often have problems such as slow response speed and poor cycle stability.
[0004] Therefore, the development of new composite fiber materials that can comprehensively utilize multiple thermal management mechanisms and have rapid response, efficient thermal conductivity, precise temperature regulation and good cycle stability has become the focus and difficulty of current research. Summary of the invention
[0005] It is based on this background that the present invention proposes a temperature-responsive composite fiber material and a preparation method thereof, aiming to solve the technical problems of how to achieve the synergistic effect of temperature response, thermal conductivity enhancement and phase change temperature regulation; how to improve the temperature response speed and sensitivity of the material; how to ensure that the material maintains stable performance during repeated use; and how to maintain good mechanical properties and processing properties of the fiber while ensuring functionality.
[0006] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a temperature-responsive composite fiber material, wherein the composite fiber material comprises the following components in parts by weight: 60-80 parts of poly (N-isopropylacrylamide); 0.5-5 parts of graphene; 10-20 parts of octadecane; 5-10 parts of n-hexadecane; 0.5-2 parts of N,N'-methylenebisacrylamide; and 0.1-0.5 parts of ammonium persulfate.
[0007] Specifically, the graphene sheet has a thickness of less than 10 nm, a lateral size of 1-5 μm, and a specific surface area of more than 500 m2 / g.
[0008] Specifically, the purity of the octadecane is greater than 99%, the phase change temperature is 28±0.5° C., and the phase change latent heat is greater than 230 J / g.
[0009] The method for preparing the temperature-responsive composite fiber material comprises the following steps:
[0010] (1) First, 0.5-5 parts by weight of graphene is added to 100-150 parts by weight of deionized water, and ultrasonically treated at 0-4° C. for 30-60 minutes to obtain a graphene suspension;
[0011] (2) Secondly, 60-80 parts by weight of N-isopropyl acrylamide monomer, 0.5-2 parts by weight of N,N'-methylenebisacrylamide and 0.1-0.5 parts by weight of ammonium persulfate are dissolved in 100-150 parts by weight of deionized water at 4°C;
[0012] (3) Then, the solutions of step (1) and (2) are mixed and reacted at 58-62° C. for 4-6 hours under a nitrogen atmosphere;
[0013] (4) Again, the resulting solution was allowed to stand at 4° C. for 12-24 hours to form a hydrogel;
[0014] (5) Further, freeze-drying the hydrogel to obtain a porous aerogel;
[0015] (6) wherein 10-20 parts by weight of octadecane and 5-10 parts by weight of n-hexadecane are dissolved in 40-60 parts by weight of anhydrous ethanol, and the aerogel is immersed therein for 12-24 hours;
[0016] (7) Then, dry in a vacuum oven at 30°C for 8-12 hours;
[0017] (8) Next, the obtained composite material is added into 200-300 parts by weight of N,N-dimethylformamide, and stirred and dissolved at 60° C. for 6-8 hours to obtain a spinning solution;
[0018] (9) Finally, fibers were prepared by wet spinning.
[0019] Specifically, in step (1), the power of the ultrasonic treatment is 300-500W.
[0020] Specifically, in step (3), the purity of nitrogen is greater than 99.99%, the flow rate is 50-100 mL / min, and the stirring speed is maintained at 300-400 rpm during the reaction.
[0021] Specifically, in step (5), the freeze-drying conditions are -50°C, 0.1 Pa, and the drying time is 48-72 hours.
[0022] Specifically, in step (6), the immersion process is maintained at a constant temperature of 40°C.
[0023] Specifically, in step (9), the specific parameters of wet spinning are as follows: spinneret aperture is 0.1-0.3 mm; spinning pressure is 0.2-0.5 MPa; coagulation bath is 50-70 wt % DMF aqueous solution; coagulation bath temperature is 20-25° C.; coagulation time is 30-60 seconds.
[0024] Specifically, the method further includes the following post-treatment steps: washing the fiber with deionized water at 30-50°C for 3-5 times, each time for 15-20 minutes; thermally stretching the fiber at 80-100°C with a stretching ratio of 1.5-2.5 times; and thermally setting the fiber at 120-140°C for 10-15 minutes.
[0025] The present invention proposes a temperature-responsive composite fiber material based on poly (N-isopropylacrylamide) (PNIPAM), graphene and phase change material (PCM). The material achieves the synergistic effect of multiple thermal management mechanisms through a carefully designed component ratio and preparation process.
[0026] Specifically, PNIPAM provides a temperature-sensitive foundation, and its rapid conformational changes near the critical temperature cause the fiber to shrink and expand. Graphene forms an efficient thermal conductivity network, which not only improves the overall thermal conductivity of the material, but also becomes denser as PNIPAM shrinks, further enhancing the thermal conductivity at high temperatures. PCM provides additional temperature regulation capabilities through the phase change process, and also provides a buffer for the phase change of PNIPAM, making the temperature change smoother.
[0027] The synergy of these multiple mechanisms brings the following beneficial effects:
[0028] 1. Ultra-high temperature responsiveness: The material exhibits rapid and significant contraction or expansion when the temperature changes, with a maximum shrinkage rate of 12%.
[0029] 2. Adaptive thermal conductivity: The thermal conductivity increases significantly with increasing temperature and can reach 0.79W / mK at 40°C, which is much higher than that of single-component materials.
[0030] 3. Accurate temperature control: The phase change process of PCM provides an additional temperature buffer for the system, making the temperature change smoother and more controllable.
[0031] 4. Excellent cycle stability: After 100 temperature cycles, the material can still maintain more than 95% of its initial performance.
[0032] 5. Good mechanical properties: The material exhibits moderate strength and ductility at different temperatures, ensuring its reliability in practical applications.
[0033] 6. Dynamic regulation of microstructure: The microstructure of the material can automatically adjust with temperature changes. This adaptive behavior provides new ideas for the design of smart materials.
[0034] In summary, the temperature-responsive composite fiber material proposed in the present invention successfully solves many problems existing in the prior art through the synergistic effect of multiple thermal management mechanisms, and provides an efficient and reliable new material solution for the fields of personal thermal management, smart textiles and energy-saving applications. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0036] The working mechanism of the temperature-responsive composite fiber material of the present invention is as follows:
[0037] 1. Temperature response mechanism: Poly (N-isopropylacrylamide) (PNIPAM) has a lower critical solution temperature (LCST) of about 32°C. When the temperature is lower than the LCST, PNIPAM forms hydrogen bonds with water molecules, becomes hydrophilic, and absorbs surrounding water to cause the polymer chain to stretch; when the temperature is higher than the LCST, the hydrophobic interactions within and between molecules are enhanced, PNIPAM becomes hydrophobic, and the polymer chain shrinks and repels water. This phase change behavior causes a reversible change in the microstructure of the material, thereby dynamically adjusting its thermal conductivity.
[0038] 2. Thermal management mechanism: At low temperatures (<32°C): PNIPAM absorbs water and expands, increasing the distance between fibers, reducing thermal conductivity, and improving the warmth retention effect. At the same time, the expanded PNIPAM network partially blocks the continuous thermal conduction channel of graphene, further reducing the thermal conductivity of the material. At high temperatures (>32°C): PNIPAM shrinks, the distance between fibers decreases, and the graphene network becomes tighter, improving thermal conductivity and promoting heat dissipation. The shrinking PNIPAM network makes the contact between graphene particles closer, forming more heat conduction paths.
[0039] 3. Latent heat regulation: Octadecane, as a phase change material (PCM), undergoes a solid-liquid phase transition at around 28°C, absorbing or releasing latent heat (about 230 J / g), further regulating the temperature. When the ambient temperature rises, octadecane melts and absorbs heat, slowing down the temperature rise; when the ambient temperature drops, octadecane solidifies and releases heat, slowing down the temperature drop. This phase change process provides additional temperature buffering capacity for the entire system. The phase change temperature of octadecane is about 28°C, while the phase change temperature of n-hexadecane is about 18°C. This combination can provide a wider phase change temperature range (18-28°C), enabling the material to provide effective thermal regulation under a wider range of temperature conditions. The composite use of the two materials can increase the overall phase change latent heat and enhance the thermal regulation ability of the material. The low phase change temperature of n-hexadecane can begin to absorb heat before PNIPAM reaches its LCST (about 32°C), providing a buffer for the phase change of PNIPAM and making the temperature response smoother. The mixing of the two alkanes affects each other's crystallization behavior, can form a more stable eutectic system, and improve the cyclic stability of the material. By adjusting the ratio of octadecane to n-hexadecane, the phase transition temperature range of the composite material can be precisely controlled. The total PCM content (15-30 parts by weight) affects the overall phase transition latent heat and thermal regulation ability of the material. The crystal morphology of the PCM affects the heat conduction path and works synergistically with the graphene network to affect the overall thermal conductivity of the material.
[0040] 4. Synergistic effect: Graphene provides a basic thermal conductivity network, significantly enhancing the overall thermal conductivity of the material. The high thermal conductivity (about 3000-5000W / mK) and two-dimensional sheet structure of graphene provide a preferential channel for heat transfer. The temperature response behavior of PNIPAM dynamically adjusts the density of the graphene network. At high temperatures, PNIPAM shrinks to make graphene particles more compact, forming more heat conduction paths; at low temperatures, PNIPAM expands to partially cut off the graphene network, reducing the efficiency of heat conduction. PCM (octadecane and n-hexadecane) fine-tune the temperature during the phase change process, forming a dual regulation mechanism with the response of PNIPAM. The phase change latent heat absorption or release process of PCM provides a buffer period for the conformational change of PNIPAM, making the temperature response of the entire system smoother and more durable. N,N'-methylenebisacrylamide, as a cross-linking agent, enhances the mechanical strength and stability of the PNIPAM network, while also affecting the porosity and temperature response sensitivity of the network. The appropriate degree of cross-linking ensures the structural stability of the material without excessively inhibiting the temperature response behavior of PNIPAM.
[0041] 5. Multi-scale thermal regulation: Molecular level: hydrophobic and hydrophilic transitions of PNIPAM molecular chains (<1nm scale); Nanoscale: changes in the thermal conductivity network formed by graphene sheets (1-5μm); Meter scale: phase change process of PCM (octadecane) particles (about 1-10μm); This multi-scale thermal regulation mechanism ensures that the material can respond effectively in different temperature ranges and achieve fine temperature control.
[0042] 6. Structure-performance relationship: Graphene content (0.5-5 parts by weight) affects basic thermal conductivity. The higher the content, the better the thermal conductivity, but too high a content will affect the flexibility of the fiber. PNIPAM content (60-80 parts by weight) determines the intensity of the temperature response. The higher the content, the more obvious the temperature response, but it may also affect the loading amount of PCM. PCM content (15-30 parts by weight) affects the latent heat regulation ability. The higher the content, the stronger the temperature buffering capacity, but it may reduce the mechanical strength of the fiber. The crosslinker content (0.5-2 parts by weight) affects the stability and response sensitivity of the network structure. Too low a content will lead to structural instability, and too high a content will inhibit the temperature response.
[0043] 7. Effect of fiber structure on performance: The fiber structure formed in the wet spinning process has an important influence on the material properties. The fiber diameter (determined by the spinneret of 0.1-0.3mm) affects the specific surface area and thermal response speed. Finer fibers are conducive to rapid thermal response, but may reduce mechanical strength. The hot stretching process (stretching ratio 1.5-2.5 times) enhances the orientation of the fiber and improves the anisotropy of mechanical properties and thermal conductivity. The heat setting process (120-140℃, 10-15 minutes) stabilizes the fiber structure and ensures the stability of long-term performance.
[0044] This composite fiber material automatically adjusts its thermal conductivity and thermal capacity under different temperature conditions through the synergistic effect of multiple mechanisms, thereby providing more precise and efficient thermal comfort regulation. The material component ratio and preparation process parameters can be optimized according to specific application requirements to obtain the best temperature regulation performance.
[0045] Example 1
[0046] The present embodiment provides a temperature-responsive composite fiber material, whose components include: the composite fiber material includes the following components in parts by weight: 60-80 parts of poly N-isopropyl acrylamide; 0.5-5 parts of graphene; 10-20 parts of octadecane; 5-10 parts of n-hexadecane; 0.5-2 parts of N,N'-methylenebisacrylamide; and 0.1-0.5 parts of ammonium persulfate.
[0047] The preparation method of the composite fiber material comprises the following steps:
[0048] First, 0.5 parts by weight of graphene (sheet thickness 8 nm, lateral size 1 μm, specific surface area 550 m 2 / g) was added into 100 parts by weight of deionized water, and ultrasonically treated at 0°C with a power of 300 W for 30 minutes to obtain a uniformly dispersed graphene suspension.
[0049] Next, 60 parts by weight of N-isopropylacrylamide monomer, 0.5 parts by weight of N,N'-methylenebisacrylamide and 0.1 parts by weight of ammonium persulfate were dissolved in 100 parts by weight of deionized water at 4° C., with a stirring speed of 300 rpm for 10 minutes until completely dissolved.
[0050] Then, the two solutions were mixed and reacted at 58°C for 4 hours under a nitrogen atmosphere with a purity of 99.99% and a flow rate of 50 mL / min. The stirring speed was maintained at 300 rpm during the reaction. In this step, N-isopropylacrylamide was polymerized under the initiation of ammonium persulfate to form a temperature-responsive polymer network, and N,N'-methylenebisacrylamide was used as a cross-linking agent to enhance the stability of the network structure.
[0051] Again, the resulting solution was allowed to stand at 4°C for 12 hours to form a hydrogel.
[0052] Furthermore, the hydrogel was pre-frozen in a -40°C refrigerator for 2 hours, and then freeze-dried at -50°C, 0.1 Pa for 48 hours to obtain a porous aerogel. In this step, the freeze-drying process retains the porous structure of the hydrogel, providing sufficient space for the subsequent loading of phase change materials.
[0053] Among them, 10 parts by weight of octadecane (purity 99.5%, phase change temperature 27.5°C, latent heat of phase change 235J / g) and 5 parts by weight of n-hexadecane (purity 99.5%, phase change temperature 18°C, latent heat of phase change 236J / g) are dissolved in 40 parts by weight of anhydrous ethanol, and heated to 40°C to completely dissolve them. The aerogel is soaked in it for 12 hours, during which the temperature is kept at 40°C. In this step, the composite phase change material is evenly distributed in the pores of the polymer network, providing the composite material with a wider range and more efficient temperature regulation ability.
[0054] Subsequently, the impregnated sample was taken out and dried in a vacuum oven at 30°C for 8 hours until the weight no longer changed.
[0055] Next, the obtained composite material was added into 200 parts by weight of N,N-dimethylformamide and dissolved under stirring at 60° C. for 6 hours to obtain a spinning solution.
[0056] Finally, a wet spinning machine was used to extrude the spinning solution through a spinneret with a diameter of 0.1 mm and a spinning pressure of 0.2 MPa. The fiber was immersed in a 50 wt% DMF aqueous solution for coagulation, with a coagulation bath temperature of 20° C. and a residence time of 30 seconds.
[0057] Preferably, in the embodiment of the present invention, the following post-treatment steps are also included: washing the fiber with deionized water at 30°C for 3 times, each time for 15 minutes; then heat stretching at 80°C with a stretching ratio of 1.5 times; and finally heat setting at 120°C for 10 minutes. These post-treatment steps further optimize the structure and performance of the fiber and improve its mechanical strength and temperature responsiveness.
[0058] Example 2
[0059] This embodiment provides another temperature-responsive composite fiber material, the components of which include: 70 parts by weight of poly N-isopropyl acrylamide, 2.75 parts by weight of graphene, 15 parts by weight of octadecane, 7.5 parts by weight of n-hexadecane, 1.25 parts by weight of N,N'-methylenebisacrylamide, and 0.3 parts by weight of ammonium persulfate.
[0060] The preparation method of the composite fiber material comprises the following steps:
[0061] First, 2.75 parts by weight of graphene (sheet thickness 5 nm, lateral size 3 μm, specific surface area 750 m 2 / g) was added into 125 parts by weight of deionized water, and ultrasonic treatment was performed at 400 W power at 2° C. for 45 minutes to obtain a uniformly dispersed graphene suspension.
[0062] Next, 70 parts by weight of N-isopropylacrylamide monomer, 1.25 parts by weight of N,N'-methylenebisacrylamide and 0.3 parts by weight of ammonium persulfate were dissolved in 125 parts by weight of deionized water at 4° C., with a stirring speed of 400 rpm for 12 minutes until completely dissolved.
[0063] Then, the two solutions were mixed and reacted at 60° C. for 5 hours in a nitrogen atmosphere with a purity of 99.995% and a flow rate of 75 mL / min. The stirring speed was maintained at 350 rpm during the reaction.
[0064] Again, the resulting solution was allowed to stand at 4°C for 18 hours to form a hydrogel.
[0065] Furthermore, the hydrogel was pre-frozen in a -40°C refrigerator for 3 hours, and then freeze-dried at -50°C and 0.1 Pa for 60 hours to obtain a porous aerogel.
[0066] Among them, 15 parts by weight of octadecane (purity 99.7%, phase change temperature 28°C, latent heat of phase change 240 J / g) and 7.5 parts by weight of n-hexadecane (purity 99.7%, phase change temperature 18.2°C, latent heat of phase change 237 J / g) were dissolved in 50 parts by weight of anhydrous ethanol and heated to 40°C to completely dissolve them. The aerogel was immersed in it for 18 hours, during which the temperature was kept constant at 40°C.
[0067] Subsequently, the immersed sample was taken out and dried in a vacuum oven at 30°C for 10 hours until the weight no longer changed.
[0068] Next, the obtained composite material was added into 250 parts by weight of N,N-dimethylformamide and dissolved under stirring at 60° C. for 7 hours to obtain a spinning solution.
[0069] Finally, a wet spinning machine was used to extrude the spinning solution through a spinneret with a diameter of 0.2 mm and a spinning pressure of 0.35 MPa. The fiber was coagulated by immersing it in a 60 wt % DMF aqueous solution with a coagulation bath temperature of 22.5° C. and a residence time of 45 seconds.
[0070] Preferably, in an embodiment of the present invention, the following post-treatment steps are also included: washing the fiber with deionized water at 40°C for 4 times, each time for 17 minutes; then heat stretching at 90°C with a stretching ratio of 2 times; and finally heat setting at 130°C for 12 minutes.
[0071] In this embodiment, the content of graphene is increased, which helps to improve the thermal conductivity of the composite fiber. At the same time, the proportion of octadecane is increased to enhance the phase change temperature adjustment ability of the material. The content of N,N'-methylenebisacrylamide is also increased, which can enhance the stability of the polymer network, but still maintain sufficient flexibility to adapt to temperature changes.
[0072] Example 3
[0073] The present embodiment provides a temperature-responsive composite fiber material, whose components include: 80 parts by weight of poly (N-isopropylacrylamide), 5 parts by weight of graphene, 20 parts by weight of octadecane, 10 parts by weight of n-hexadecane, 2 parts by weight of N,N'-methylenebisacrylamide and 0.5 parts by weight of ammonium persulfate.
[0074] The preparation method of the composite fiber material comprises the following steps:
[0075] First, 5 parts by weight of graphene (sheet thickness 2 nm, lateral size 5 μm, specific surface area 1000 m 2 / g) was added into 150 parts by weight of deionized water, and ultrasonically treated at 4°C with a power of 500 W for 60 minutes to obtain a uniformly dispersed graphene suspension.
[0076] Next, 80 parts by weight of N-isopropylacrylamide monomer, 2 parts by weight of N,N'-methylenebisacrylamide and 0.5 parts by weight of ammonium persulfate were dissolved in 150 parts by weight of deionized water at 4° C., with a stirring speed of 500 rpm for 15 minutes until completely dissolved.
[0077] Then, the two solutions were mixed and reacted at 62°C for 6 hours in a nitrogen atmosphere with a purity of 99.999% and a flow rate of 100 mL / min. The stirring speed was maintained at 400 rpm during the reaction. In this step, the high concentration of monomers and cross-linking agents helps to form a denser polymer network, while the high content of graphene can form a more continuous heat conduction channel.
[0078] Again, the resulting solution was allowed to stand at 4°C for 24 hours to form a hydrogel.
[0079] Furthermore, the hydrogel was pre-frozen in a -40°C freezer for 4 hours and then freeze-dried at -50°C, 0.1 Pa for 72 hours to obtain a porous aerogel. The extended freeze-drying time ensured the complete formation of the porous structure.
[0080] Among them, 20 parts by weight of octadecane (purity 99.9%, phase transition temperature 28.5°C, latent heat of phase change 245J / g) and 10 parts by weight of n-hexadecane (purity 99.9%, phase transition temperature 18.5°C, latent heat of phase change 238J / g) were dissolved in 60 parts by weight of anhydrous ethanol and heated to 40°C to completely dissolve them. The aerogel was soaked in it for 24 hours, during which the temperature was kept at 40°C. The extended soaking time helps octadecane to penetrate more fully into the polymer network.
[0081] Subsequently, the immersed sample was taken out and dried in a vacuum oven at 30°C for 12 hours until the weight no longer changed.
[0082] Next, the obtained composite material was added into 300 parts by weight of N,N-dimethylformamide and dissolved under stirring at 60° C. for 8 hours to obtain a spinning solution.
[0083] Finally, a wet spinning machine was used to extrude the spinning solution through a spinneret with a diameter of 0.3 mm and a spinning pressure of 0.5 MPa. The fiber was coagulated by immersing it in a 70 wt % DMF aqueous solution with a coagulation bath temperature of 25° C. and a residence time of 60 seconds.
[0084] Preferably, in the embodiment of the present invention, the following post-treatment steps are also included: washing the fiber with deionized water at 50°C for 5 times, each time for 20 minutes; then heat stretching at 100°C with a stretching ratio of 2.5 times; and finally heat setting at 140°C for 15 minutes. These more intensive post-treatment steps help to further improve the mechanical strength and temperature response performance of the fiber.
[0085] Example 4
[0086] The present embodiment provides a temperature-responsive composite fiber material, whose components include: 75 parts by weight of poly (N-isopropylacrylamide), 3.5 parts by weight of graphene, 16 parts by weight of octadecane, 9 parts by weight of n-hexadecane, 1.5 parts by weight of N,N'-methylenebisacrylamide and 0.4 parts by weight of ammonium persulfate.
[0087] The preparation method of the composite fiber material comprises the following steps:
[0088] First, 3.5 parts by weight of graphene (sheet thickness 4 nm, lateral size 4 μm, specific surface area 800 m 2 / g) was added into 135 parts by weight of deionized water, and ultrasonically treated at 450 W power at 3°C for 50 minutes to obtain a uniformly dispersed graphene suspension.
[0089] Next, 75 parts by weight of N-isopropylacrylamide monomer, 1.5 parts by weight of N,N'-methylenebisacrylamide and 0.4 parts by weight of ammonium persulfate were dissolved in 135 parts by weight of deionized water at 4° C., with a stirring speed of 450 rpm for 13 minutes until they were completely dissolved.
[0090] Then, the two solutions were mixed and reacted at 61°C for 5.5 hours under a nitrogen atmosphere with a purity of 99.997% and a flow rate of 85 mL / min. The stirring speed was maintained at 375 rpm during the reaction. This moderate reaction condition is intended to balance the formation of the polymer network and the dispersion of graphene.
[0091] Again, the resulting solution was allowed to stand at 4°C for 20 hours to form a hydrogel.
[0092] Furthermore, the hydrogel was pre-frozen in a -40°C refrigerator for 3.5 hours and then freeze-dried at -50°C and 0.1 Pa for 65 hours to obtain a porous aerogel.
[0093] Among them, 16 parts by weight of octadecane (purity 99.8%, phase transition temperature 28.2°C, latent heat of phase change 242 J / g) and 9 parts by weight of n-hexadecane (purity 99.8%, phase transition temperature 18.3°C, latent heat of phase change 237.5 J / g) were dissolved in 55 parts by weight of anhydrous ethanol and heated to 40°C to completely dissolve them. The aerogel was immersed in it for 20 hours, during which the temperature was kept constant at 40°C.
[0094] Subsequently, the immersed sample was taken out and dried in a vacuum oven at 30°C for 11 hours until the weight no longer changed.
[0095] Next, the obtained composite material was added into 275 parts by weight of N,N-dimethylformamide and dissolved under stirring at 60° C. for 7.5 hours to obtain a spinning solution.
[0096] Finally, the spinning solution was extruded through a spinneret with a diameter of 0.25 mm using a wet spinning machine, and the spinning pressure was 0.4 MPa. The fiber was immersed in a 65 wt% DMF aqueous solution for coagulation, the coagulation bath temperature was 23.5° C., and the residence time was 52 seconds.
[0097] Preferably, in an embodiment of the present invention, the following post-treatment steps are also included: washing the fiber with deionized water at 45°C for 4 times, each time for 18 minutes; then heat stretching at 95°C with a stretching ratio of 2.2 times; and finally heat setting at 135°C for 13 minutes.
[0098] In this embodiment, the ratio of each component and the process parameters are selected at a moderate level to achieve the best balance of temperature responsiveness, thermal conductivity and mechanical properties. This balance helps the fiber to show excellent comprehensive performance in practical applications.
[0099] Comparative Example 1
[0100] This comparative example provides a temperature-responsive fiber material without graphene, the components of which include: 60 parts by weight of poly-N-isopropylacrylamide, 10 parts by weight of octadecane, 5 parts by weight of n-hexadecane, 0.5 parts by weight of N,N'-methylenebisacrylamide and 0.1 parts by weight of ammonium persulfate. The preparation method is the same as that of Example 1, but the graphene dispersion step is omitted.
[0101] This comparative example is intended to verify the importance of graphene in composite fibers. The lack of graphene leads to a significant reduction in the thermal conductivity of the material, thereby affecting the efficiency and speed of the temperature response. This illustrates the key role of graphene in providing a thermally conductive network and confirms the synergistic effect of graphene and other components in the present invention.
[0102] Comparative Example 2
[0103] This comparative example provides a temperature-responsive composite fiber material without a phase change material, the components of which include: 70 parts by weight of poly-N-isopropylacrylamide, 2.75 parts by weight of graphene, 1.25 parts by weight of N,N'-methylenebisacrylamide, and 0.3 parts by weight of ammonium persulfate. The preparation method is the same as that of Example 2, but the phase change material impregnation step is omitted.
[0104] This comparative example is intended to illustrate the importance of phase change materials in temperature regulation. Without phase change materials, the material will lose additional temperature buffering capacity, resulting in a temperature response that is not smooth and durable enough. This verifies the synergistic effect of PCM and temperature responsive polymer in the present invention.
[0105] Comparative Example 3
[0106] This comparative example provides an over-crosslinked temperature-responsive composite fiber material, the components of which include: 80 parts by weight of poly-N-isopropylacrylamide, 5 parts by weight of graphene, 20 parts by weight of octadecane, 10 parts by weight of n-hexadecane, 4 parts by weight of N,N'-methylenebisacrylamide, and 0.5 parts by weight of ammonium persulfate. The preparation method is the same as that of Example 3, but the amount of N,N'-methylenebisacrylamide is increased to 4 parts by weight.
[0107] This comparative example is intended to demonstrate the negative impact of excessive crosslinking on material performance. Too high a degree of crosslinking will inhibit the temperature response behavior of PNIPAM and reduce the sensitivity and response speed of the material. This demonstrates the importance of optimizing the amount of crosslinking agent used in the present invention for balancing structural stability and responsiveness.
[0108] Comparative Example 4
[0109] This comparative example provides a temperature-responsive composite fiber material with excessively high graphene content, the components of which include: 75 parts by weight of poly-N-isopropylacrylamide, 10 parts by weight of graphene, 16 parts by weight of octadecane, 9 parts by weight of n-hexadecane, 1.5 parts by weight of N,N'-methylenebisacrylamide and 0.4 parts by weight of ammonium persulfate. The preparation method is the same as that of Example 4, but the amount of graphene is increased to 10 parts by weight.
[0110] This comparative example is intended to illustrate that too high a graphene content may lead to a decrease in the flexibility of the material, affecting the processability and comfort of the fiber. This verifies the importance of optimizing the amount of graphene in the present invention for balancing thermal conductivity and fiber flexibility.
[0111] Comparative Example 5
[0112] This comparative example provides a temperature-responsive composite fiber material without ultrasonic dispersion, and its components are the same as those in Example 1. The preparation method is also the same as that in Example 1, but in the graphene dispersion step, only mechanical stirring is used without ultrasonic treatment.
[0113] This comparative example is intended to demonstrate the importance of ultrasonic dispersion for the uniform distribution of graphene in the polymer matrix. Without ultrasonic treatment, graphene may agglomerate, resulting in a discontinuous thermal network, thereby affecting the overall performance of the material. This verifies the necessity of process parameter optimization in the present invention.
[0114] Comparative Example 6
[0115] This comparative example provides a temperature-responsive composite fiber material without post-treatment, and its components are the same as those of Example 2. The preparation method is also the same as that of Example 2, but all post-treatment steps (washing, heat stretching and heat setting) are omitted.
[0116] This comparative example is intended to illustrate the importance of the post-treatment step for optimizing fiber structure and performance. Without post-treatment, the fiber may have residual solvent, poor structural stability, and affected mechanical properties and temperature response performance. This proves the key role of the post-treatment process in the present invention in improving the comprehensive performance of the material.
[0117] Through these comparative examples, we have fully verified the synergistic mechanism of the components in the present invention and the importance of process parameter optimization. These comparative examples cover the key endpoint values and intermediate values in the formula, fully demonstrating the creativity of the present invention in component design and process optimization. Each comparative example is specifically compared with the corresponding embodiment, which strongly proves the superiority of the composite fiber material of the present invention in terms of temperature responsiveness, thermal conductivity, mechanical properties and processing performance.
[0118] In order to comprehensively evaluate the effectiveness and superiority of the present invention, we designed a series of experiments. The following is a detailed experimental design and result analysis. The evaluation method is designed as follows:
[0119] 1. Temperature responsiveness test: We designed a test device that simulates the microenvironment of human skin. The fiber sample was placed in a constant temperature and humidity chamber with the initial temperature set at 25°C and relative humidity at 40%. The temperature was then raised to 40°C at a rate of 1°C / min, while the relative humidity was raised to 90% to simulate the sweating process. The length change and thermal conductivity change of the fiber were recorded throughout the process.
[0120] 2. Thermal conductivity test: The thermal conductivity of the fiber was measured using the transient plane heat source method (TPS). The test was conducted at two temperature points, 25°C and 40°C, to evaluate the effect of temperature on thermal conductivity.
[0121] 3. Phase change latent heat and temperature regulation ability test: Differential scanning calorimetry (DSC) was used to measure the phase change temperature and latent heat of the composite fiber. The heating rate was 5°C / min and the temperature range was 0-50°C. At the same time, an infrared thermal imager was used to record the cooling curve of the fiber on simulated human skin (35°C).
[0122] 4. Mechanical properties test: The breaking strength and breaking elongation of the fiber were tested using a universal material testing machine at two temperature points: 25°C and 40°C. The tensile rate was 50 mm / min.
[0123] 5. Microstructure analysis: Scanning electron microscopy (SEM) was used to observe the surface morphology and cross-sectional structure of the fibers. Energy dispersive spectroscopy (EDS) was used to determine the distribution of graphene and PCM in the fibers.
[0124] 6. Cyclic stability test: The fiber sample is cycled between 25°C and 40°C for 100 times, with each temperature change lasting 30 minutes. The temperature responsiveness, thermal conductivity and mechanical property changes before and after the test cycle are tested.
[0125] The experimental results are shown in the following table:
[0126] Table 1. Temperature responsiveness and thermal conductivity test results
[0127]
[0128]
[0129] Table 2. Phase change performance and mechanical properties test results
[0130]
[0131] The results are analyzed as follows:
[0132] 1. Temperature responsiveness: Examples 1-4 all exhibited excellent temperature responsiveness, showing significant shrinkage when the temperature rose. Among them, Example 3 performed best, with a shrinkage rate of 12%. In contrast, due to excessive cross-linking, the shrinkage rate of Comparative Example 3 was only 3%, indicating that the degree of cross-linking has a significant effect on temperature responsiveness.
[0133] 2. Thermal conductivity: Examples 1-4 all show a significant increase in thermal conductivity when the temperature rises, which is related to the shrinkage of PNIPAM and the densification of the graphene network. Comparative Example 1 has significantly poor thermal conductivity due to the lack of graphene, confirming the key role of graphene in improving thermal conductivity.
[0134] 3. Phase change performance: Examples 1-4 all showed good phase change performance, and the phase change temperature was between 28-29°C, which was in line with the comfortable temperature range for the human body. The latent heat of phase change increased with the increase of PCM content, and Example 3 performed the best. Comparative Example 2 did not show phase change performance due to the lack of PCM.
[0135] 4. Mechanical properties: Examples 1-4 exhibit good mechanical properties at both 25°C and 40°C. It is worth noting that the breaking strength of all samples at 40°C decreased slightly, but the breaking elongation increased, which is related to the temperature responsiveness of PNIPAM. Comparative Example 3 exhibits higher breaking strength but lower breaking elongation due to excessive crosslinking.
[0136] 5. Microstructure analysis (SEM and EDS results): Examples 1-4 all show uniform fiber structures, with graphene and PCM evenly distributed. Comparative Example 5, due to the lack of ultrasonic dispersion, observed obvious graphene agglomeration, which explains its poor thermal conductivity.
[0137] 6. Cyclic stability: After 100 temperature cycles, the temperature responsiveness, thermal conductivity and mechanical properties of Examples 1-4 all remained above 95% of the initial values, showing excellent cyclic stability. In contrast, due to the lack of post-processing steps, the performance of Comparative Example 6 decreased significantly after the cyclic test, and only maintained about 80% of the initial value.
[0138] According to the comprehensive performance evaluation, Example 3 performs best. It has the highest temperature responsiveness (shrinkage rate 12%), the best thermal conductivity (thermal conductivity coefficient 0.79W / mK at 40°C), the highest phase change latent heat (70J / g), and excellent mechanical properties and cycle stability. This excellent performance is due to its optimized component ratio and preparation process:
[0139] 1. The higher PNIPAM content (80 parts by weight) ensures strong temperature responsiveness.
[0140] 2. An appropriate amount of graphene (5 parts by weight) provides an excellent thermal conductive network without affecting the flexibility of the fiber.
[0141] 3. A higher PCM content (30 parts by weight) brings about a significant phase change temperature regulation effect.
[0142] 4. A moderate degree of cross-linking (2 parts by weight of cross-linking agent) ensures structural stability without excessively inhibiting the responsiveness of PNIPAM.
[0143] Unexpected technical effects:
[0144] 1. Super synergistic effect: The performance of Example 3 far exceeds the simple superposition effect of each single component. For example, its thermal conductivity at 40°C (0.79 W / mK) is higher than the sum of Comparative Example 1 (no graphene, 0.22 W / mK) and Comparative Example 2 (no PCM, 0.65 W / mK). This shows that there is a strong synergistic effect between PNIPAM, graphene and PCM, which may be due to the shrinkage of PNIPAM making the graphene network more dense, while the phase change process of PCM provides an additional driving force for the conformational change of PNIPAM.
[0145] 2. Adaptability of temperature regulation: Experimental results show that the thermal conductivity of the fiber increases significantly with increasing temperature (such as from 0.50 to 0.79 W / mK in Example 3). This adaptive behavior means that the material can dissipate heat faster when the temperature rises, and retain heat when the temperature drops, forming an intelligent self-regulating system.
[0146] 3. Temperature dependence of mechanical properties: All examples showed lower breaking strength but higher breaking elongation at 40°C. This property may be due to the enhanced hydrophobicity of PNIPAM at high temperatures, making the fiber structure more flexible. This property can provide additional comfort and safety in practical applications.
[0147] 4. Dynamic changes in microstructure: Although SEM analysis cannot be directly observed, the comprehensive performance test results suggest that the microstructure of the fiber is dynamically adjusted with temperature changes. This dynamic structural change may be a direct reflection of the synergistic effect of the components, providing important inspiration for the development of new smart materials.
[0148] 5. Improved cycle stability: The excellent cycle stability of Examples 1-4 exceeded expectations, which may be due to the stabilization of the PNIPAM structure by the graphene network and the buffering effect of PCM on temperature fluctuations. This feature greatly extends the service life of the material and improves its practical application value.
[0149] In summary, the temperature-responsive composite fiber material of the present invention achieves excellent temperature responsiveness, thermal conductivity, phase change temperature regulation ability and mechanical properties through the synergistic effect of PNIPAM, graphene and PCM. This multifunctional integration not only brings about a significant improvement in various performances, but also produces a series of unexpected synergistic effects and adaptive behaviors. These characteristics make the material have broad application prospects in the fields of personal thermal management, smart textiles and energy efficiency. Future research can further explore these synergistic mechanisms and provide important guidance for the development of a new generation of smart materials.
[0150] The above description is only an embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A temperature-responsive composite fiber material, characterized in that: The composite fiber material comprises the following components in parts by weight: 60-80 parts of poly N-isopropyl acrylamide; 0.5-5 parts of graphene; 10-20 parts of octadecane; 5-10 parts of n-hexadecane; 0.5-2 parts of N,N'-methylenebisacrylamide; and 0.1-0.5 parts of ammonium persulfate.
2. The temperature-responsive composite fiber material according to claim 1, characterized in that: The graphene sheet has a thickness of less than 10 nm, a lateral size of 1-5 μm, and a specific surface area of more than 500 m 2 / g.
3. The temperature-responsive composite fiber material according to claim 1, characterized in that: The purity of the octadecane is greater than 99%, the phase change temperature is 28±0.5°C, and the phase change latent heat is greater than 230 J / g.
4. The method for preparing a temperature-responsive composite fiber material according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) First, 0.5-5 parts by weight of graphene is added to 100-150 parts by weight of deionized water, and ultrasonically treated at 0-4° C. for 30-60 minutes to obtain a graphene suspension; (2) Secondly, 60-80 parts by weight of N-isopropyl acrylamide monomer, 0.5-2 parts by weight of N,N'-methylenebisacrylamide and 0.1-0.5 parts by weight of ammonium persulfate are dissolved in 100-150 parts by weight of deionized water at 4°C; (3) Then, the solutions of step (1) and (2) are mixed and reacted at 58-62° C. for 4-6 hours under a nitrogen atmosphere; (4) Again, the resulting solution was allowed to stand at 4° C. for 12-24 hours to form a hydrogel; (5) Further, freeze-drying the hydrogel to obtain a porous aerogel; (6) wherein 10-20 parts by weight of octadecane and 5-10 parts by weight of n-hexadecane are dissolved in 40-60 parts by weight of anhydrous ethanol, and the aerogel is immersed therein for 12-24 hours; (7) Then, dry in a vacuum oven at 30°C for 8-12 hours; (8) Next, the obtained composite material is added into 200-300 parts by weight of N,N-dimethylformamide, and stirred and dissolved at 60° C. for 6-8 hours to obtain a spinning solution; (9) Finally, the fibers were prepared by wet spinning.
5. The preparation method according to claim 4, characterized in that: In the step (1), the power of the ultrasonic treatment is 300-500W.
6. The preparation method according to claim 4, characterized in that: In the step (3), the purity of nitrogen is greater than 99.99%, the flow rate is 50-100 mL / min, and the stirring speed is maintained at 300-400 rpm during the reaction.
7. The preparation method according to claim 4, characterized in that: In the step (5), the freeze-drying conditions are -50°C, 0.1 Pa, and the drying time is 48-72 hours.
8. The preparation method according to claim 4, characterized in that: In the step (6), the immersion process is maintained at a constant temperature of 40°C.
9. The preparation method according to claim 4, characterized in that: In the step (9), the specific parameters of wet spinning are as follows: the spinneret aperture is 0.1-0.3 mm; the spinning pressure is 0.2-0.5 MPa; the coagulation bath is a 50-70 wt % DMF aqueous solution; the coagulation bath temperature is 20-25° C.; and the coagulation time is 30-60 seconds.
10. The preparation method according to claim 4, characterized in that: The method also includes the following post-treatment steps: washing the fiber with deionized water at 30-50°C for 3-5 times, each time for 15-20 minutes; thermally stretching the fiber at 80-100°C with a stretching ratio of 1.5-2.5 times; and thermally setting the fiber at 120-140°C for 10-15 minutes.
Citation Information
Cited By
Graphene cloth analysis method and system based on observation of temperature fluctuation
CN120275439A