Wood fiber softening penetrant and preparation method thereof

By using penetrants synthesized by alkyl glycosides in lime fiber pulping, the chemical mechanical pulping process is optimized, and the problems of high power consumption and poor mechanical properties in lime fiber pulping process are solved, and efficient fiber softening and electricity are achieved The consumption is reduced, improving the fineness and mechanical properties of the slurry.

CN119021021AActive Publication Date: 2024-11-26SHANDONG YAXUN KANGDE FINE CHEM CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411441763.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-11-26
Estimated Expiration
2044-10-16

AI Technical Summary

Technical Problem

In the prior art, wood fiber pulping process has high power consumption, high slurry fineness, poor paper mechanical properties, and the fibers are not fully softened, resulting in high power consumption and severe stress damage to fibers. The penetrant on the market is used to deal with wood. The material effect is not ideal and the slurry quality is low.

Method used

The permeable agent is synthesized by alkyl glycosides as the main raw material. By changing the ratio, dosage and ratio of the permeable agent and the permeable agent, the molecular weight of polyethylene glycol and the polymerization degree of alkyl glycosides are controlled, and the pH value is adjusted in combination with phosphoric acid, using 3- (2,3-epoxypropoxy)propyltrimethoxysilol and other components were prepared, Kant KDHG-S518 penetrant, used for pulping of eucalyptus, poplar and trench, and optimized chemical mechanical pulping process. Reduce power consumption, improve fiber humidity and tensile index.

Benefits of technology

Effectively reduce the electrical energy consumption of chemical mechanical pulping, improve the wet weight of fibers and tensile index, enhance the fineness and mechanical properties of the slurry, improve the loose thickness and tensile index of the paper, and ensure the high slurry Quality and energy-saving effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119021021A_ABST
    Figure CN119021021A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of pulping and papermaking, in particular to a wood fiber softening penetrant and a preparation method thereof. According to the invention, the problems of poor permeation effect, high power consumption and poor slurry quality of the penetrant in the chemical mechanical pulping preparation process are solved. The high-quality slurry is prepared by the following steps of: dipping raw materials, defibering, performing first-stage pre-dipping, defibering, adding a substance containing a penetrant, performing second-stage pre-dipping, performing first-stage pulping, performing first-stage low-concentration pulping, performing second-stage low-concentration pulping and the like. By using the synthetic penetrant I, the power consumption of the slurry is reduced, and the tensile index is integrally improved; by changing the proportion of the penetrant I and the penetrant II and changing the type and proportion of the penetrant II, the average power consumption per ton of slurry is reduced; by changing the dosage of the penetrant and changing the conditions of the preimpregnation stage and the defibering conditions, the fineness of the pulp is increased, the bulk of paper prepared from the pulp is reduced, and the mechanical property is improved; and the power consumption is reduced by changing the type and dosage of the defoaming agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pulping and papermaking, in particular to a wood fiber softening penetrant and a preparation method thereof. Background Art

[0002] With the progress of the times and the improvement of living standards, people have higher and higher demands for the quality of paper. The raw materials of paper include wood fiber, plant fiber and various fibers. These fibers are pulped after pre-treatment to further prepare paper. The quality of pulp is closely related to the pre-treatment steps. The main components of wood fiber include cellulose, hemicellulose, lignin and extracts. The pre-treatment is mainly to remove hemicellulose, lignin, etc., so as to improve the quality of pulp. The commonly used substance in pre-treatment is penetrant. The quality of penetrant has a direct positive relationship with the quality of the prepared pulp.

[0003] Penetrants are additives that promote the rapid wetting of the fiber or fabric surface by water, improve the surface tension of the liquid phase, increase fluidity, and penetrate into the fiber, and promote the penetration of substances such as sodium hydroxide into the fiber. The requirements that penetrants need to meet are resistance to hard water and alkali, and strong permeability. The raw materials for making paper are various fiber raw materials. The fiber raw materials must first be chopped and boiled to make pulp. Due to the different compositions and chemical components of these fiber materials, the penetrant cannot achieve good penetration, the wood chip fiber cannot be softened well, the yield and efficiency of pulp fiber are low, and the power consumption increases, and the energy saving is poor.

[0004] To overcome the above technical problems, patent CN115262256B discloses a small molecule fiber penetration softener and a preparation method thereof, using sugar, alcohol, acid, alkali, modifier and other materials as small molecule fiber penetration softener, first with glucose containing highly active hemiacetal hydroxyl as raw material, with ethanol / n-butanol under the action of a catalyst, acetal reaction occurs, the prepared small molecule surfactant is compounded with N-methylmorpholine oxide and fast penetrant T to obtain the penetration softener. The penetration softener can reduce the effect of the surface tension of the impregnation liquid, and the acetal product of the small molecule can penetrate into the fiber interior, which is conducive to the subsequent fiber separation and pulping, and the use amount of the chemical liquid is also reduced. However, the freeness of the fiber is high, the water filterability is poor, and the drug impregnation effect is reduced.

[0005] The literature Jinglin T, Ziyan H, Yongxiang M, et al. Synthesis and Surface Properties of Polyether-Based Silicone Surfactants with Different Siloxane Groups [J]. Journal of Surfactants and Detergents, 2019, 22 (4): 875-883. discloses a polyether-based silicone surfactant containing different siloxane groups. This surfactant has good penetration and can significantly reduce the surface tension of water, but has poor degradation performance and poor environmental protection.

[0006] Patent CN113174770B discloses a method for pretreating poplar fibers by using a penetrant in conjunction with phosphoric acid impregnation and coupled steam explosion, wherein the crushed poplar wood chips are impregnated into a mixed impregnation solution containing a penetrant and a phosphoric acid solution, mixed evenly and impregnated, and then blasted and post-treated to complete the raw material processing process, wherein the penetrant used is a condensate of ethylene oxide and a higher fatty alcohol, which has a good penetration effect, is easy to operate, low cost, and high efficiency, and the penetrant promotes a large amount of hemicellulose degradation in the poplar fibers, improves the problems of large fiber diameter, large pulp fineness, poor mechanical properties of paper prepared from pulp, and low tensile index.

[0007] In the prior art, there are problems such as high power consumption, high pulp fineness, and poor mechanical properties of paper made of pulp when penetrants are used in the pulping process of wood materials. In addition, due to the low temperature and small amount of alkali used in the production process of chemical mechanical pulping, the raw materials cannot be fully softened, resulting in high power consumption, serious damage to the fibers due to stress, and low pulp quality. Similar products on the market have unsatisfactory actual penetration effects on wood materials and non-wood materials, and the pulp quality is low.

[0008] Therefore, a wood fiber softening penetrant and a preparation method thereof are proposed. Summary of the invention

[0009] The object of the present invention is to provide a wood fiber softening penetrant and a preparation method thereof. Penetrant one is synthesized by using alkyl glycoside as the main raw material. The penetrant prepared by penetrant one is applied to pulping of eucalyptus, poplar and eucalyptus, the power consumption of pulp is reduced, the fiber moisture is increased, and the tensile index is improved as a whole; by changing the ratio of penetrant one to penetrant two, changing the type and proportion of penetrant two, the average power consumption per ton of pulp is reduced; by changing the amount of penetrant, changing the temperature, time and debonding conditions of the pre-impregnation stage, the pulp fineness is increased, the bulk thickness of paper made of pulp is reduced, and the mechanical properties are improved; by changing the type, amount and proportion of the defoaming agent, the power consumption is reduced.

[0010] To achieve the above object, the present invention provides the following technical solutions:

[0011] In one aspect, the present invention provides a method for preparing a wood fiber softening penetrant, comprising the following steps:

[0012] The maleic anhydride solution is heated and refluxed, and then cooled to obtain a maleic acid aqueous solution; phosphoric acid is used to adjust the pH of the maleic acid aqueous solution to 3, and then 10.0-12.0 parts of polyethylene glycol are added thereto to obtain a mixed solution; the mixed solution is heated and refluxed for 1 hour to obtain a maleic acid polyethylene glycol ester solution; the polyethylene glycol has an average molecular weight of 200-1000;

[0013] Dissolving an alkyl glycoside in deionized water to obtain an alkyl glycoside solution; adding p-toluenesulfonic acid and the maleic acid polyethylene glycol ester solution to the alkyl glycoside solution to obtain a penetrant precursor solution; adding 3-(2,3-epoxypropoxy)propyltrimethoxysilanol and concentrated sulfuric acid to the penetrant precursor solution, continuing the reaction, filtering, and vacuum drying to obtain a penetrant; the alkyl glycoside has a polymerization degree n=1.1-3.0;

[0014] The penetrant one and the penetrant two are mixed in a volume ratio of 1-9:3-13, and stirred and mixed at 60°C to obtain a light yellow viscous liquid; the mixture is cooled to room temperature to prepare the Kant KDHG-S518 penetrant, i.e. the wood fiber softening penetrant; the components of the penetrant two are any three of sodium salt of dioctyl sulfonatesuccinate, fatty alcohol polyoxyethylene ether, isooctyl alcohol polyoxyethylene ether phosphate, sodium linear alkylbenzene sulfonate, fatty alcohol polyoxyalkyl ether, and alkyl trimethyl ammonium salt; the volume ratio of the components of the penetrant two is 1-7:1-5:2-8.

[0015] Alkyl polyglycoside nonionic surfactants have the properties of both ionic and anionic surfactants, good foaming properties (rich and delicate foam), strong alkali and electrolyte resistance, good surface activity, and better degradability compared to conventional polymer surfactants. It is a "green" functional surfactant. By modifying its surface and introducing polyethylene glycol and hydrolyzed epoxy silane, its penetration into wood raw materials is further improved, and the good absorption of drugs by wood materials is enhanced.

[0016] The hydrophilicity of polyethylene glycol and alkyl glycoside and the lipophilicity of 3-(2,3-epoxypropoxy)propyltrimethoxysilanol constitute the main body of penetrant one. The amphiphilic functional groups are effectively combined, and the molecular weight of polyethylene glycol and the degree of polymerization of alkyl glycoside are controlled at the same time, so that the molecular weight of penetrant one is within a reasonable range. If the molecular weight is small, the penetration is incomplete, and if the molecular weight is large, the penetration resistance is enhanced, so that all-round three-dimensional wetting is achieved within an appropriate range and the penetration process is promoted.

[0017] Preferably, the preparation method of the 3-(2,3-epoxypropoxy)propyltrimethoxysilanol is as follows: the deionized water, methanol and 29.7 parts of propylene glycol are mixed to obtain a mixed solvent; 3-(2,3-epoxypropoxy)propyltrimethoxysilane is added to the mixed solvent, the pH of the system is adjusted to 4.0 using phosphoric acid, and then stirred at room temperature until the system becomes transparent after 30 minutes, and then the system is dried to remove water and organic solvent to obtain the 3-(2,3-epoxypropoxy)propyltrimethoxysilanol.

[0018] Preferably, the polymerization degree of the alkyl glycoside is n=1.4-2.4, and the polyethylene glycol is one of PEG200, PEG300, PEG400, PEG600 and PEG1000.

[0019] Preferably, the degree of polymerization of the fatty alcohol polyoxyethylene ether is 3 or 9.

[0020] On the other hand, the present invention provides a wood fiber softening penetrant, which is Kant KDHG-S518 penetrant; the wood fiber softening penetrant includes penetrant one and penetrant two; the volume ratio of penetrant one to penetrant two is 1-9:3-13; the components of penetrant two are any three of sodium salt of dioctyl sulfonatesuccinate, fatty alcohol polyoxyethylene ether, isooctyl alcohol polyoxyethylene ether phosphate, sodium linear alkylbenzene sulfonate, fatty alcohol polyoxyalkyl ether, and alkyl trimethyl ammonium salt; the volume ratio of the components of penetrant two is 1-7:1-5:2-8.

[0021] Preferably, the application of the wood fiber softening penetrant in chemical mechanical pulping; the steps of the chemical mechanical pulping are as follows: the raw material is impregnated with hot water; after the impregnation, a first stage of extrusion and deflaking is performed; after the first stage of extrusion and deflaking, a first stage of pre-impregnation is performed; after the first stage of pre-impregnation, a second stage of extrusion and deflaking is performed; after the second stage of extrusion and deflaking, a second stage of pre-impregnation is performed; after the second stage of pre-impregnation, a first stage of refining, a second stage of refining, latent elimination, screening, and beating are performed to obtain pulp; the second stage of refining includes a first stage of low-concentration refining and a second stage of low-concentration refining; the first stage of extrusion and deflaking and the second stage of pre-impregnation are performed The screw compression ratio of the first stage extrusion decomposition is 2-6:1; the material-liquid ratio of the raw material and the hot water for impregnation is 1:6.5; the temperature of the first stage pre-impregnation is 80-90°C, and the time is 60-90min; in terms of percentage of 1 ton of slurry, the amount of penetrant in the second stage pre-impregnation is 0.50%-1.02%, the amount of defoamer is 0.10%-0.32%, the amount of sodium hydroxide is 1.5%, the amount of sodium silicate is 1.2%, the amount of hydrogen peroxide is 1.6%, the amount of DTPA chelating agent is 0.005%, the temperature is 55-70°C, and the time is 30-40min.

[0022] Preferably, the raw material is any one, two or three of eucalyptus, poplar, alder, birch, acacia, straw, sorghum stalks and corn stalks.

[0023] Preferably, the defoamer is obtained by mixing an alcohol defoamer, a phosphoric acid defoamer and a silicone defoamer in a mass ratio of 1-4:1-3:1.

[0024] Preferably, the alcohol defoamer is any one of fatty alcohol defoamer, high carbon alcohol defoamer, ethanol, and n-propanol; the phosphoric acid defoamer is any one of tributyl phosphate and triisobutyl phosphate; the organosilicon defoamer is any one of pulp black liquor defoamer and general-purpose organosilicon defoamer.

[0025] Preferably, the wood fiber softening penetrant is prepared by any one of the above preparation methods; using the wood fiber softening penetrant, the average power consumption per ton of pulp of eucalyptus as raw material is 920-929KWh / admt, the average fiber wet weight is 1.40-1.51, and the average tensile index is 18.6-21.5cm 3 / g; the average power consumption of a ton of pulp made of poplar wood is 912-920KWh / admt, the average fiber wet weight is 1.28-1.43, and the average tensile index is 19.3-22.4cm 3 / g; the average power consumption of 1 ton of pulp with wood as raw material is 908-917KWh / admt, the average fiber wet weight is 1.30-1.48, and the average tensile index is 19.0-21.7cm 3 / g; the average power consumption per ton of pulp with birch as raw material is 1031.2-1038.5KWh / admt; the proportion of fibers larger than 50 mesh in high-concentration pulp with straw, sorghum stalks and corn stalks as raw materials is 24.7%-28.5%, the Canadian freeness is 782-794mL, and the whiteness is 25.99%-26.50%; the proportion of fibers larger than 50 mesh in the second-stage low-concentration pulp with straw, sorghum stalks and corn stalks as raw materials is 4.26%-4.87%, and the paper bulk is 2.20-2.58cm 3 / g, the paper tensile index is 22.6-27.1N·m / g, the first-stage low-concentration mill outlet power is 2198-2205KW, and the second-stage low-concentration mill outlet power is 1128-1153KW; the Canadian freeness of the pulp using eucalyptus and acacia as raw materials is 402-418mL, and the power consumption is 673-690KW·h.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. By using alkyl glycoside as the main raw material and grafting it on the surface to synthesize a grafted penetrant, it has a good penetration effect on eucalyptus, poplar and eucalyptus. By reacting maleic anhydride, polyethylene glycol and 3-(2,3-epoxypropoxy)propyltrimethoxysilanol with alkyl glycoside to polymerize, controlling the molecular weight and dosage of polyethylene glycol, and controlling the molecular polymerization degree of alkyl glycoside, the synthesized penetrant has a good penetration effect on a variety of wood materials during the chemical mechanical pulping process. The power consumption of chemical mechanical pulping is reduced. When the beating degree is constant, the pulp fiber has a large wet weight, a high tensile index, and a high strength.

[0028] 2. The present invention prepares an alkyl polyglycoside nonionic polymer penetrant, and uses it in combination with penetrant 2 to improve the penetration effect of the penetrant, so that the plant fiber is easily softened. To reduce the mechanical resistance of harder fibers during the pulping process, more current supply is required to overcome the corresponding resistance. By controlling the volume ratio between penetrant 1 and penetrant 2, controlling the type of penetrant 2 and the volume ratio of each component of penetrant 2, it is ensured that the power consumption is reduced while the pulping quality remains stable, thereby achieving the effect of energy saving.

[0029] 3. The present invention controls the screw compression ratio, the amount of penetrant used, and the temperature and impregnation time of the first and second pre-impregnation stages during the extrusion and decomposition process, so that the proportion of fibers larger than 50 mesh that have been retained at a high concentration is reduced, and the diameter of the fibers is reduced, which is beneficial to the subsequent pulping process and improves the fineness of the pulp, but has no obvious effect on the freeness and whiteness of the pulp.

[0030] 4. The present invention pressurizes and degrades the wood material before pre-impregnation, controls the use conditions of the de-impregnation equipment, reasonably controls the amount of penetrant during the second-stage pre-impregnation process, and selects appropriate pre-impregnation temperature and pre-impregnation time. This reduces the fineness and bulk of the pulp from the second-stage low-concentration refining, and improves the tensile index. In addition, under the premise of ensuring the quality of the pulp, the outlet power of the second-stage low-concentration grinding can be appropriately reduced.

[0031] 5. The present invention controls the addition ratio of the defoamer in the prepreg stage, controls the types and ratios of the components in the defoamer, avoids the generation of large and small foams during the addition of the penetrant and other substances and during the stirring process, thereby making the penetration process stable. The prepared slurry has a reduced freeness, a moderate freeness, and good water filtration performance. In addition, the power consumption is reduced, and the process is energy-saving. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The results of the bulk and tensile index of the two-stage pulp paper of Examples 25-32 of the present invention are shown in FIG.

[0033] Figure 2This is a diagram of power consumption results of Example 58 of the present invention;

[0034] Figure 3 The figure is a flow chart of the pulping process of the present invention. DETAILED DESCRIPTION

[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] See also Figures 1 to 3 The present invention provides a wood fiber softening penetrant and a preparation method thereof, and the technical scheme is as follows:

[0037] The substance information involved in the present invention is as follows:

[0038] 3-(2,3-Epoxypropoxy)propyltrimethoxysilane CAS: 2530-83-8; p-Toluenesulfonic acid CAS: 104-15-4; Sulfosuccinic acid dioctyl sodium salt CAS: 1639-66-3; 2-isooctanol polyoxyethylene ether phosphate CAS: 68439-39-4; Sodium linear alkylbenzene sulfonate CAS: 25155-30-0; Alkyl trimethyl ammonium salt CAS: 85409-24-1; Tributyl phosphate C AS: 126-73-8; triisobutyl phosphate CAS: 126-71-6; fatty alcohol polyoxyethylene ether (N=3) (AEO-3), fatty alcohol polyoxyalkyl ether, fatty alcohol polyoxyethylene ether (N=9) (AEO-9) were all purchased from BASF Chemical Co., Ltd.; high carbon alcohol defoamer, fatty alcohol defoamer, pulp black liquor defoamer were all purchased from Foshan Nanhai Datian Chemical Co., Ltd.; general-purpose silicone defoamer was purchased from Hubei Chengfeng Chemical Co., Ltd.;

[0039] Example 1

[0040] The preparation method of penetrant 1 is as follows:

[0041] 9.9 parts of maleic anhydride and 100 parts of deionized water are added to a round-bottom flask, and 0.1 parts of potassium hydroxide are added thereto, and mixed evenly to obtain a maleic anhydride solution; the temperature is raised to 80°C, refluxed for 100 minutes, and cooled to obtain a maleic acid aqueous solution; phosphoric acid is used to adjust the pH of the maleic acid aqueous solution to 3, and then polyethylene glycol (average molecular weight 200) is added thereto to obtain a mixed solution; the mixed solution is heated to 115°C, and the reflux reaction is continued for 1 hour to obtain a maleic acid polyethylene glycol ester solution.

[0042] 31.0 parts of deionized water, 15.8 parts of methanol, and 29.7 parts of propylene glycol are mixed to obtain a mixed solvent; 23.6 parts of 3-(2,3-epoxypropoxy)propyltrimethoxysilane are added to the mixed solvent, and the pH of the system is adjusted to 4.0 using phosphoric acid, and then stirred at room temperature until the system becomes transparent after 30 minutes, and then the system is dried to remove water and organic solvents to obtain 3-(2,3-epoxypropoxy)propyltrimethoxysilanol.

[0043] Dissolve 10 parts of alkyl glycoside (polymerization degree n=1.2) in 100 parts of deionized water to obtain an alkyl glycoside solution; transfer the alkyl glycoside solution to a high-temperature and high-pressure reactor, add 1.2 parts of p-toluenesulfonic acid and maleic acid polyethylene glycol ester solution, and react at 110°C for 1.5 hours to obtain a penetrant precursor solution; add 19.5 parts of 3-(2,3-epoxypropoxy)propyltrimethoxysilanol and 1.5 parts of concentrated sulfuric acid to the penetrant precursor solution, continue to increase the temperature to 120°C, stir and react for 5 hours to obtain a penetrant intermediate solution; cool the penetrant intermediate solution to room temperature, then filter and vacuum dry to obtain a penetrant. All reactions were carried out under nitrogen protection.

[0044] The penetrant is a mixture of penetrant 1 and penetrant 2 in a volume ratio of 3:7; penetrant 2 is prepared from sodium dioctyl sulfonate succinate, AEO-3, and isooctyl alcohol polyoxyethylene ether phosphate in a volume ratio of 1:1:2. After penetrant 1 and penetrant 2 are mixed, they are stirred at 60°C to obtain a light yellow viscous liquid; the mixture is cooled to room temperature to obtain Kant KDHG-S518 penetrant, i.e., a wood fiber softening penetrant.

[0045] The overall process flow of the penetrant is as follows: Figure 3 As shown: the raw materials are impregnated with hot water (solid-liquid ratio 1:6.5), followed by one-stage extrusion decomposition (screw compression ratio of 4.5:1), one-stage pre-impregnation (sodium hydroxide 10Kg / ton pulp, sodium silicate 12Kg / ton pulp, hydrogen peroxide 13Kg / ton pulp, DTPA0.5Kg / ton pulp, 80℃, 90min), two-stage extrusion decomposition (screw compression ratio of 4.5:1), two-stage pre-impregnation (penetrant 6.0Kg / ton pulp, defoamer 1.2Kg / ton pulp, sodium hydroxide 15Kg / ton pulp, sodium silicate 12Kg / ton pulp, hydrogen peroxide 16Kg / ton pulp, chelating agent DTPA0.5Kg / ton pulp, 70℃, 45min), one-stage refining, two-stage refining (one-stage low-concentration refining, two-stage low-concentration refining), de-latching, screening, beating, sheet making, and performance testing.

[0046] Example 2-12

[0047] Comparative Examples 1-3

[0048] Different from Example 1, the detailed information of the preparation process of Example is shown in Table 1.

[0049] Table 1 Preparation method of penetrant 1

[0050]

[0051]

[0052] Embodiment 13

[0053] The penetrants prepared in Examples 1-12 and Comparative Examples 1-3 were applied to the chemical mechanical pulping process for a small test. The test time was from 16:00 on August 26, 2022 to 23:00 on August 28, 2022. The raw materials were 1000kg eucalyptus, 1000kg poplar and 1000kg eucalyptus respectively. The on-site production conditions were 700 tons / day, and the penetrant was added continuously by using a metering pump. The power consumption, fiber wet weight (when the beating degree is 25) and tensile index of the test process were recorded. The tensile index was determined according to GB / T 12914-2018 "Constant tension method (20mm / min) for the determination of tensile strength of paper and paperboard". The test results are shown in Table 2.

[0054] Table 2 Test results of penetrants of Examples 1-12 and Comparative Examples 1-3

[0055]

[0056]

[0057] The penetrant prepared by the present invention is used in the chemical mechanical pulping process, such as Figure 3 After the penetrant is applied, the average power consumption per ton of pulp of eucalyptus wood as raw material is 920-929KWh / admt, the average fiber wet weight is 1.40-1.51, and the average tensile index is 18.6-21.5cm 3 / g; the average power consumption of a ton of pulp made of poplar wood is 912-920KWh / admt, the average fiber wet weight is 1.28-1.43, and the average tensile index is 19.3-22.4cm 3 / g; the average power consumption of 1 ton of pulp with wood as raw material is 908-917KWh / admt, the average fiber wet weight is 1.30-1.48, and the average tensile index is 19.0-21.7cm 3 / g. Before and two days after the addition of the penetrant, the average power consumption per ton of pulp for the three wood materials was higher than that in the example, and the average fiber wet weight and the average tensile index were lower. The results of Examples 1-3 show that by changing the amount of polyethylene glycol, the average power consumption per ton of pulp and the average fiber wet weight and the average tensile index changed. The results of Examples 2, 4-7 show that with the increase of the molecular weight of polyethylene glycol, the average power consumption per ton of pulp did not change significantly, and the average fiber wet weight and the average tensile index showed a trend of first increasing and then decreasing. The results of Examples 6, 8-12 show that when the degree of polymerization of alkyl polyglycoside is controlled within the range of 1.4-2.4, the power consumption and pulp strength change. In Comparative Example 1, the molecular weight of polyethylene glycol is too large, resulting in the average power consumption per ton of pulp not changing significantly compared with the groups two days before and two days after the addition of the penetrant, and the average fiber wet weight and the average tensile index did not increase much. In Comparative Examples 2 and 3, the degree of polymerization of alkyl polyglycoside is too high or too low, which will make the pulp strength increase insignificantly. In summary, the embodiment and the comparative example have lower power consumption and higher pulp strength than the group two days before and two days after the addition of the penetrant. The average tensile index of poplar wood is the highest compared with eucalyptus and eucalyptus, and the average fiber wet weight of eucalyptus wood is the highest compared with poplar wood and eucalyptus.

[0058] Examples 14-23

[0059] Different from Example 9, the following preparation conditions are changed, as shown in Table 3.

[0060] Table 3 Components and dosage ratio of penetrant 1 and penetrant 2

[0061]

[0062] Comparative Example 4

[0063] Different from Example 14, only penetrant 1 was added as the penetrant.

[0064] Comparative Example 5

[0065] The difference from Example 14 is that the penetrant is added in a prepreg stage.

[0066] Embodiment 24

[0067] The penetrants obtained in Example 9, Examples 14-23 and Comparative Examples 4 and 5 were used for the preparation of chemical mechanical pulping of birch, and the pilot process was as follows: On June 3 at 10:00, Kurita 1203 penetrant (dosage was 0.8 kg / t pulp) was used online, and on June 8 at 14:00, the penetrants of the examples and comparative examples were switched respectively. During the experiment, the pulping quality remained stable, and only the process parameters were adjusted, and the equipment with large energy consumption was recorded in real time, including the 1# main mill, the 2# main mill, the 1# low-concentration mill, the 2# low-concentration mill, and the slag pulp mill.

[0068] The power consumption results are shown in Table 4, and the specific recorded data of Example 14 is shown in Table 5.

[0069] Table 4 Power consumption results of the embodiments and comparative examples

[0070] Average power consumption per ton of pulp (KWh / admt) Embodiment 14 1032.3 Embodiment 15 1034.0 Example 16 1034.8 Embodiment 17 1035.0 Embodiment 18 1032.1 Embodiment 19 1033.6 Embodiment 20 1033.0 Embodiment 21 1031.2 Embodiment 22 1032.0 Embodiment 23 1038.5 Comparative Example 4 1044.7 Comparative Example 5 1040.0 Kurita 1203 1045.8

[0071] Table 5 Specific test data of Example 14

[0072]

[0073]

[0074]

[0075] In the process of chemical mechanical pulping, the average power consumption per ton of pulp is in the range of 1031.2-1038.5 KWh / admt by using the penetrant prepared by the examples and comparative examples. The results of Examples 14-16 show that the power consumption gradually increases by changing the proportion of the components in penetrant 2. The sodium salt of dioctyl sulfonate succinate is mainly an anionic surfactant, in which the sulfonated succinic acid can react with the moisture on the fiber surface, and the ester can enter the interior of the fiber, thereby reducing the surface tension, promoting the penetration and dispersion of substances such as sodium hydroxide and hydrogen peroxide, promoting the decomposition of non-wood fiber substances such as sugars and lignin in wood materials, and promoting the decomposition of wood fibers. AEO-3 is a condensation product of fatty alcohol and ethylene oxide, isooctyl alcohol polyoxyethylene ether phosphate, both of which are non-ionic surfactants, and synergistically act with penetrant 1 to improve the penetration ability of fibers. The results of Examples 14, 17-19 show that by increasing the proportion of penetrant one, the average power consumption per ton of pulp first decreases and then increases. It can be seen that the volume ratio of penetrant one to penetrant two needs to be controlled within a reasonable range. The results of Examples 14 and 20 show that the use of sodium dioctyl sulfonated succinate in penetrant two consumes less power, which may be due to the special composition of its structure compared with linear sodium alkylbenzene sulfonate, which makes it more permeable. The results of Examples 14, 21-23 show that when isooctyl alcohol polyoxyethylene ether phosphate is replaced, when alkyl trimethyl ammonium salt is used, the power consumption increases. Alkyl trimethyl ammonium salt is a cationic surfactant. The ammonium salt adheres to the surface of the wood material, hindering the wetting process, thereby reducing the effect of penetration. Combined with the data in Table 5, it can be seen that the power consumption is significantly reduced when Kurita 1203 penetrant is used in the first half and the penetrant prepared by the present invention is used in the second half. Comparative Example 4 only adds penetrant one as a penetrant, and the power consumption increases compared with the embodiment. In Comparative Example 5, the penetrant was added in a pre-preg section too early, resulting in decreased penetration effect and increased power consumption.

[0076] Examples 25-42

[0077] Comparative Example 6

[0078] Different from Example 21, the following preparation conditions are changed, as shown in Table 6.

[0079] Table 6 Changes in conditions during the preparation process

[0080]

[0081]

[0082] Embodiment 43

[0083] According to the methods of Examples 25-42 and Comparative Example 6, the chemical mechanical pulp prepared from the raw materials (15% rice straw + 45% sorghum stalks + 40% corn stalks) was graded for freeness, whiteness and fiber, and the penetrant was added continuously at a flow rate of 170 mL / min to test the quality of the high-concentration refining section pulp.

[0084] The freeness of the pulp suspension was measured by a Canadian standard freeness tester, where the pulp suspension was diluted to a concentration of 0.3% and the temperature was 20.5°C. The whiteness was measured in accordance with GB / T 7974-2002 "Determination of brightness (whiteness) of paper, paperboard and pulp (diffuse / vertical method)", and the instrument was a WS-SD colorimetric whiteness meter manufactured by Wenzhou Instrument Co., Ltd. The test results are shown in Table 7. The specific results of the test process of Example 32 and Comparative Example 6 are shown in Tables 8 and 9.

[0085] Table 7 Fiber ratio, freeness and whiteness test results

[0086]

[0087]

[0088] In the embodiment, the proportion of fibers with a mesh size of >50 at the outlet of the high-concentration refining section (i.e., the high-concentration pulp after the first refining) is 24.7%-28.5%, the Canadian freeness is 782-794mL, and the whiteness is 25.99%-26.50%. The results show that by controlling the amount of penetrant, the compression ratio of the first extrusion decompression screw, the first pre-impregnation temperature and time, and the second pre-impregnation temperature and time, there is no significant effect on the freeness and whiteness of the pulp, but the pulp fineness is improved. The possible reason is that the whiteness of the pulp is related to the amount of hydrogen peroxide used, and the freeness of the pulp is related to the wood raw material used and the instrument parameters of the pulper, so the performance has no obvious change. However, the proportion of fibers with a mesh size of >50 is reduced. In Examples 25-32, as the amount of penetrant is gradually increased, the proportion of fibers with a mesh size of >50 is gradually reduced. The increase in the amount of penetrant increases the softness of the wood pulp, and sodium hydroxide and other substances are easily infiltrated therein, making it easier to break under the same mechanical force, thereby reducing the diameter of the fiber and increasing the fineness. In Comparative Example 6, no penetrant is added, the penetration effect decreases, and the hardness of the wood material increases, so the fiber diameter increases after pulping. The results of Examples 32-36 show that by changing the compression ratio of a first-stage extrusion decomposition screw, the fineness is minimized when the ratio of Example 34 is 6:1. The results of Examples 34 and 37-42 show that by controlling the pre-impregnation time and temperature of the first and second stages, the permeability of the penetrant and other components is enhanced, thereby reducing the fineness of the slurry. Combined with the results of Table 8, it can be seen that the freeness and whiteness of the slurry are in a dynamic change process as a whole. After being treated with the penetrant and conditions of Example 32 of the present invention, the freeness is reduced and the whiteness is increased, but the change is not significant. The results in Table 9 show that the overall fineness is reduced under the conditions of Example 32.

[0089] Table 8 Specific results of freeness and whiteness of Example 32 and Comparative Example 6

[0090]

[0091] Table 9 Results of fiber classification and >50 mesh ratio of Example 32 and Comparative Example 6

[0092]

[0093] Embodiment 44

[0094] The raw materials (15% rice straw + 45% sorghum stalks + 40% corn stalks) were processed according to the methods of Examples 25-42 and Comparative Example 6 to prepare the chemical mechanical pulp, and the power consumption, bulk, strength and ratio of fixed-size fibers of the first and second stage refining were tested. The penetrant was added in a continuous manner at a flow rate of 170 mL / min. The pulp was prepared into paper, and the thickness and strength were measured according to the method of GB / T 24323-2009 "Pulp·Laboratory Paper·Determination of Physical Properties". The test results are shown in Table 10. The bulk and tensile index results of the second stage pulp of Examples 25-32 are shown in Table 10. Figure 1 The basic information of power consumption during the test of Example 32 and Comparative Example 6 is shown in Table 11, and the fiber diameter information at the outlet of the second-stage low-concentration grinding mill is shown in Table 12.

[0095] Table 10 Test results of slurry physical properties of Examples 25-42 and Comparative Example 6

[0096]

[0097] The proportion of the second-stage low-concentration pulp>50 mesh in the present invention is 4.26%-4.87%, and the paper bulk thickness is 2.20-2.58cm 3 / g, the paper tensile index is 22.6-27.1N·m / g, the outlet power of the first low-concentration mill is 2198-2205KW, and the outlet power of the second low-concentration mill is 1128-1153KW. The proportion of the second-stage refining pulp>50 mesh in Example 44 is much lower than that of the high-concentration mill outlet fiber>50 mesh in Example 43. As the chemical mechanical pulping preparation process proceeds, the fineness of the pulp gradually decreases. Compared with the group in Comparative Example 6 without adding a penetrant, the proportion of the second-stage refining pulp>50 mesh in Example 43 is significantly reduced. The results of the bulk thickness of the second-stage pulp in Table 10 show that as the proportion of the second-stage refining pulp>50 mesh decreases, the bulk thickness shows an overall downward trend, and the tensile index of the second-stage pulp increases instead. The pulp is prepared into paper. According to Page theory, a paper sheet is a network structure composed of random fibers. Small-sized fibers are combined more times in the same area and can be filled in the gaps of larger fibers. The structure of the paper is tighter and the strength is greater. Table 12 shows in detail the changes in pulp fineness of Comparative Example 6 and Example 32. Therefore, the bulk is reduced, the tensile index is increased, and the mechanical properties of the paper prepared by the pulp are improved. Figure 1The results show that with the increase of the amount of penetrant, the bulk decreases and the tensile index increases. The results of Examples 25-42 in Table 10 compared with the comparative example 6 without adding the penetrant group show that the outlet power of the first stage low-concentration mill has not changed significantly, but the outlet power of the second stage low-concentration mill is reduced compared with the comparative example, and the reduction value is 14-39KW. Table 11 shows the specific data of the application process of Example 32 in detail. According to the amount of penetrant added by the present invention and the control of the process conditions, the pulp fineness is increased, the power consumption is reduced, and the mechanical strength of the paper made of pulp is improved.

[0098] Table 11 Power consumption information during the test of Example 32 and Comparative Example 6

[0099]

[0100]

[0101] Table 12 Fiber diameter information of the second stage low concentration mill outlet of Example 32 and Comparative Example 6

[0102]

[0103] Examples 45-57

[0104] Comparative Examples 7-9

[0105] The defoamer is obtained by mixing three types of substances in a fixed mass ratio. Different from Example 34, the type and amount of the defoamer are changed, as shown in Table 13. The three types of substances in Table 13 are alcohol defoamers, phosphoric acid defoamers, and silicone defoamers.

[0106] Table 13 Type and dosage of defoamer

[0107]

[0108]

[0109] Embodiment 58

[0110] The defoamers prepared in Examples 45-57 and Comparative Examples 6-9 were used for high bulk chemical mechanical pulping, wherein the raw materials used were 80% eucalyptus and 20% acacia, the production capacity was 1360 tons / day, the penetrant was continuously added by a metering pump, and the test time was 2024-9-10, 08:40-2024-9-12, 08:40. The test results of freeness and power consumption are shown in Table 14. The changes in freeness and power consumption during the production process of Example 45 are shown in Table 15.

[0111] Table 14 Changes in freeness and power consumption of Examples 45-57 and Comparative Examples 7-9

[0112] Freeness(mL) Power consumption (KW·h) Embodiment 45 410 683 Embodiment 46 418 680 Embodiment 47 415 685 Embodiment 48 413 690 Embodiment 49 412 681 Embodiment 50 402 673 Embodiment 51 405 682 Embodiment 52 415 685 Embodiment 53 420 689 Embodiment 54 405 685 Embodiment 55 410 684 Embodiment 56 403 675 Embodiment 57 408 678 Comparative Example 6 428 722 Comparative Example 7 420 710 Comparative Example 8 424 715 Comparative Example 9 426 719

[0113] The results in Table 14 show that the Canadian freeness of the pulp prepared by the present invention is 402-418mL, and the power consumption is 673-690KW·h. The results of Examples 45-50 show that with the increase in the amount of defoamer, the freeness shows a trend of first increasing and then decreasing. When the amount of defoamer added in Example 50 is the highest, the freeness is the lowest, and the power consumption shows a trend of decreasing, increasing, and decreasing. In Example 45, when the amount of defoamer is the lowest, the freeness and power consumption are moderate. The results of Examples 45, 51-53 show that by using a high-carbon alcohol defoamer as the type of alcohol defoamer, as shown in Example 51, the power consumption is the lowest, the high-carbon alcohol defoamer has good compatibility with the penetrant, and the function of the penetrant is promoted. Example 54 uses triisobutyl phosphate as a phosphoric acid defoamer, which is not much different from using tributyl phosphate. The results of Examples 51 and 55 show that the effect of using a pulp black liquor defoamer is better than that of a general-purpose silicone defoamer. The results of Examples 51, 56, and 57 show that when the ratio of the three types of substances in Example 56 is 4:3:3, the power consumption is the lowest, which is 6750KW·h. Comparison of the results of Comparative Examples 6-8 with those of Example 45 shows that the power consumption and freeness are high when only one type of defoaming agent is used in the comparative examples. However, the results of Examples 45-57 and Comparative Examples 7-9 are better than the effect of Comparative Example 6 without adding a penetrant. The results in Table 15 show that the freeness and power consumption in the production process of Example 45 are lower than the effect of Comparative Example 6 without adding a penetrant.

[0114] Table 15 Changes in freeness and power consumption during the production process of Example 45

[0115]

[0116] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a wood fiber softening penetrant, characterized in that: The following steps are involved: The maleic anhydride solution is heated and refluxed, and then cooled to obtain a maleic acid aqueous solution; phosphoric acid is used to adjust the pH of the maleic acid aqueous solution to 3, and then 10.0-12.0 parts of polyethylene glycol are added thereto to obtain a mixed solution; the mixed solution is heated and refluxed for 1 hour to obtain a maleic acid polyethylene glycol ester solution; the polyethylene glycol has an average molecular weight of 200-1000; Dissolving an alkyl glycoside in deionized water to obtain an alkyl glycoside solution; adding p-toluenesulfonic acid and the maleic acid polyethylene glycol ester solution to the alkyl glycoside solution to obtain a penetrant precursor solution; adding 3-(2,3-epoxypropoxy)propyltrimethoxysilanol and concentrated sulfuric acid to the penetrant precursor solution, continuing the reaction, filtering, and vacuum drying to obtain a penetrant; the alkyl glycoside has a polymerization degree n=1.1-3.0; The penetrant one and the penetrant two are mixed in a volume ratio of 1-9:3-13, stirred and mixed at 60°C to obtain a light yellow viscous liquid; the mixture is cooled to room temperature to prepare the wood fiber softening penetrant; the components of the penetrant two are any three of dioctyl sulfonated succinate sodium salt, fatty alcohol polyoxyethylene ether, isooctyl alcohol polyoxyethylene ether phosphate, linear alkylbenzene sodium sulfonate, fatty alcohol polyoxyalkyl ether, and alkyl trimethyl ammonium salt; the volume ratio of the components of the penetrant two is 1-7:1-5:2-8.

2. The method for preparing a wood fiber softening penetrant according to claim 1, characterized in that: The preparation method of the 3-(2,3-epoxypropoxy)propyltrimethoxysilanol is as follows: the deionized water, methanol and 29.7 parts of propylene glycol are mixed to obtain a mixed solvent; 3-(2,3-epoxypropoxy)propyltrimethoxysilane is added to the mixed solvent, phosphoric acid is used to adjust the pH of the system to 4.0, and then the mixture is stirred at room temperature until the system becomes transparent after 30 minutes, and then the system is dried to remove water and organic solvent to obtain the 3-(2,3-epoxypropoxy)propyltrimethoxysilanol.

3. The method for preparing a wood fiber softening penetrant according to claim 1, characterized in that: The polymerization degree of the alkyl glycoside is n=1.4-2.4; the polyethylene glycol is one of PEG200, PEG300, PEG400, PEG600 and PEG1000.

4. The method for preparing a wood fiber softening penetrant according to claim 1, characterized in that: The polymerization degree of the fatty alcohol polyoxyethylene ether is 3 or 9.

5. A wood fiber softening penetrant, characterized in that: The wood fiber softening penetrant is Kant KDHG-S518 penetrant; the wood fiber softening penetrant includes penetrant one and penetrant two; the volume ratio of penetrant one to penetrant two is 1-9:3-13; the components of penetrant two are any three of dioctyl sulfonated succinate sodium salt, fatty alcohol polyoxyethylene ether, isooctyl alcohol polyoxyethylene ether phosphate, linear alkylbenzene sodium sulfonate, fatty alcohol polyoxyalkyl ether, and alkyl trimethyl ammonium salt; the volume ratio of the components of penetrant two is 1-7:1-5:2-8.

6. A wood fiber softening penetrant according to claim 5, characterized in that: The application of the wood fiber softening penetrant in chemical mechanical pulping; the chemical mechanical pulping steps are as follows: soaking the raw material with hot water; after the soaking, performing a stage of extrusion and deflaking; after the stage of extrusion and deflaking, performing a stage of pre-impregnation; after the stage of pre-impregnation, performing a second stage of extrusion and deflaking; After the two-stage extrusion deflaking, a two-stage pre-impregnation is performed; after the two-stage pre-impregnation, the pulp is obtained by the steps of one-stage refining, two-stage refining, delatching, screening and beating; the two-stage refining includes one-stage low-concentration refining and two-stage low-concentration refining; the screw compression ratio of the one-stage extrusion deflaking and the two-stage extrusion deflaking is 2-6:1; the material-liquid ratio of the raw material and the hot water for impregnation is 1:6.5; the temperature of the one-stage pre-impregnation is 80-90°C, and the time is 60-90min; in terms of percentage of 1 ton of pulp, the amount of penetrant in the two-stage pre-impregnation is 0.50%-1.02%, the amount of defoamer is 0.10%-0.32%, the amount of sodium hydroxide is 1.5%, the amount of sodium silicate is 1.2%, the amount of hydrogen peroxide is 1.6%, the amount of DTPA chelating agent is 0.005%, the temperature is 55-70°C, and the time is 30-40min.

7. A wood fiber softening penetrant according to claim 6, characterized in that: The raw materials are any one, two or three of eucalyptus, poplar, ebony, birch, acacia, straw, sorghum stalks and corn stalks.

8. A wood fiber softening penetrant according to claim 6, characterized in that: The defoamer is obtained by mixing an alcohol defoamer, a phosphoric acid defoamer and an organosilicon defoamer in a mass ratio of 1-4:1-3:

1.

9. A wood fiber softening penetrant according to claim 8, characterized in that: The alcohol defoamer is any one of fatty alcohol defoamer, high carbon alcohol defoamer, ethanol and n-propanol; the phosphoric acid defoamer is any one of tributyl phosphate and triisobutyl phosphate; the organosilicon defoamer is any one of pulp black liquor defoamer and general organosilicon defoamer.

10. The wood fiber softening penetrant according to claim 5, characterized in that: The wood fiber softening penetrant is prepared by any one of the preparation methods of claims 1 to 4; using the wood fiber softening penetrant, the average power consumption per ton of pulp of eucalyptus as raw material is 920-929 KWh / admt, the average fiber wet weight is 1.40-1.51, and the average tensile index is 18.6-21.5 cm 3 / g; the average power consumption of a ton of pulp made of poplar wood is 912-920KWh / admt, the average fiber wet weight is 1.28-1.43, and the average tensile index is 19.3-22.4cm 3 / g; the average power consumption of 1 ton of pulp with wood as raw material is 908-917KWh / admt, the average fiber wet weight is 1.30-1.48, and the average tensile index is 19.0-21.7cm 3 / g; the average power consumption per ton of pulp with birch as raw material is 1031.2-1038.5KWh / admt; the proportion of fibers larger than 50 mesh in high-concentration pulp with straw, sorghum stalks and corn stalks as raw materials is 24.7%-28.5%, the Canadian freeness is 782-794mL, and the whiteness is 25.99%-26.50%; the proportion of fibers larger than 50 mesh in the second-stage low-concentration pulp with straw, sorghum stalks and corn stalks as raw materials is 4.26%-4.87%, and the paper bulk is 2.20-2.58cm 3 / g, the paper tensile index is 22.6-27.1N·m / g, the first-stage low-concentration mill outlet power is 2198-2205KW, and the second-stage low-concentration mill outlet power is 1128-1153KW; the Canadian freeness of the pulp using eucalyptus and acacia as raw materials is 402-418mL, and the power consumption is 673-690KW·h.

Citation Information

Patent Citations

  • A method for enhanced pre-impregnation of chemithermomechanical pulp

    CN102268825A

  • Cooking auxiliary agent as well as preparation method and application thereof

    CN117005230A

  • Process for increasing digestion efficiency of lignocellulosic material in a treatment vessel

    US20230160140A1

  • Process for enhancing white liquor penetration into wood chips by contacting the chips with a mixture of the white liquor and a polymethylalkyl siloxane

    US5728265A

  • Pulping composition containing aminoalkoxylsilanes and a pulping process using the composition

    US6123810A