Carbon fiber high-concentration stable dispersion method
By heating and ultrasonic stirring in alkaline lignin and urea, the carbon fiber surface is modified, and the problem of poor dispersion performance of carbon fiber in water is solved, achieving efficient carbon fiber dispersion and papermaking uniformity improvement.
Patent Information
- Application Number
- CN202411304607.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-19
AI Technical Summary
Carbon fibers have poor dispersion performance in water, making it difficult to form uniform papermaking, and the bonding strength between fibers is low, making it difficult to form.
An alkali solution of alkali lignin and urea is configured, and the hydrophilic groups and rough structure of the carbon fiber surface are modified through heating and ultrasonic stirring, thereby reducing the interaction force between the fibers and achieving efficient dispersion of carbon fibers.
The dispersion uniformity of carbon fibers and the bonding strength between fibers are improved, the uniformity and stability of papermaking are enhanced, and the dispersion process is simplified.
Smart Images

Figure CN119021028A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon fiber application, and in particular to a high-concentration and stable dispersion method for carbon fibers. Background Art
[0002] As part of the proton exchange membrane fuel cell, the gas diffusion layer plays the role of supporting the catalyst layer and collecting current. At present, the first choice for the gas diffusion layer is carbon fiber paper. Carbon fiber is a super fiber material. More than 90% of the chemical composition is composed of carbon elements. It has the advantages of high conductivity, high modulus, high strength, corrosion resistance, etc. Preparation of carbon fiber paper usually can choose any one of polypropylene, asphalt, and cellulose. The fiber diameter is preferably 5-20μm and the length is preferably 4-20mm. The surface of the carbon fiber is a chaotic layer graphite structure with grooves and obvious cracks. The surface is rough, which makes the friction between the fibers larger and difficult to be dispersed into a single fiber. Carbon and carbon are connected by non-polar covalent bonds, resulting in less surface active groups on the carbon fiber, which is not easy to be wetted by water, easy to flocculate in water, and poor dispersion performance. In addition, unlike plant fibers, carbon fibers do not produce hydrogen bonds, there is no bonding strength between fibers, it is difficult to form, and there is no bonding strength between fibers, it is difficult to make paper. Therefore, improving the bonding strength between fibers is also the key to wet-making carbon fiber paper. However, due to the low surface activity of carbon fiber, it is insoluble in water, difficult to combine, and difficult to paper into shape. Therefore, the key to papermaking carbon fiber paper is to evenly disperse the carbon fiber in the water phase and improve the bonding strength between the fibers. Summary of the invention
[0003] The purpose of the present invention is to provide a method for high-concentration and stable dispersion of carbon fibers. The present invention can achieve efficient dispersion of carbon fibers and has the characteristics of being simple and convenient.
[0004] The technical solution of the present invention is a method for high-concentration and stable dispersion of carbon fibers, comprising the following steps:
[0005] Step 1, preparing an alkaline solution with a concentration of 0.5-1.5 mol / L, and adding alkali lignin to the alkaline solution to form a mixed solution; wherein the concentration of the alkali lignin in the mixed solution is 1-2 wt%;
[0006] Step 2, heating the mixed solution to 60-70° C., and then adding 0.3-0.8 wt % urea to the mixed solution to obtain a dispersion;
[0007] Step 3: Raise the temperature to 80-100° C., add the carbon fiber into the cellulose suspension and stir, and perform ultrasonic stirring for 1-3 minutes to disperse the carbon fiber.
[0008] In the above-mentioned high-concentration stable dispersion method of carbon fiber, in step 1, the alkaline solution is a sodium hydroxide solution with a concentration of 1 mol / L.
[0009] In the above-mentioned high-concentration stable dispersion method of carbon fiber, the concentration of the alkali lignin is 1.5Wt%.
[0010] In the above-mentioned high-concentration stable dispersion method of carbon fiber, in step 2, the temperature at which the mixed liquid is heated is 65°C.
[0011] In the aforementioned high-concentration stable dispersion method for carbon fibers, in step 2, the concentration of urea is 0.5 wt %.
[0012] In the aforementioned high-concentration stable dispersion method for carbon fiber, in step 3, the temperature of the ultrasonic stirring is 90°C.
[0013] In the above-mentioned high-concentration stable dispersion method of carbon fiber, in step 3, the ultrasonic stirring time is 2 minutes.
[0014] In the aforementioned high-concentration stable dispersion method for carbon fiber, in step 3, the power of the ultrasonic stirring is 500W.
[0015] In the aforementioned high-concentration stable dispersion method for carbon fibers, the length of the carbon fibers is 4-8 mm.
[0016] Compared with the prior art, the present invention first configures an alkaline solution of alkali lignin, then heats it and adds urea to form an alkali lignin-urea alkaline solution system, thereby in this system, the active groups of the alkali lignin are used to modify the carbon fibers, thereby increasing the surface hydrophilic groups and the surface roughness structure, and at the same time, under the action of heating and ultrasonic stirring, the viscosity of the alkali lignin-urea alkaline solution system decreases with the increase of temperature, thereby increasing the dispersion speed of the carbon fibers, reducing the interaction force between the carbon fibers, and reducing the internal friction between the carbon fibers, thereby achieving rapid dispersion of the carbon fibers under the influence of multiple factors. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a dispersion diagram of carbon fibers in the embodiment;
[0018] Figure 2 The statistical diagram of the uniformity of dispersed carbon fiber papermaking in Examples 3-6 and Comparative Example 2;
[0019] Figure 3 Schematic diagram of the dispersed carbon fiber stability index of Examples 3-6 and Comparative Example 2. DETAILED DESCRIPTION
[0020] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but they are not intended to limit the present invention.
[0021] Embodiment 1: A method for high-concentration and stable dispersion of carbon fibers, comprising the following steps:
[0022] Step 1, preparing an alkaline solution with a concentration of 0.5 mol / L, and adding alkali lignin to the alkaline solution to form a mixed solution; wherein the concentration of the alkali lignin in the mixed solution is 1 wt%;
[0023] Step 2, heating the mixed solution to 60° C., and then adding 0.3 wt % urea to the mixed solution to obtain a dispersion;
[0024] Step 3: Raise the temperature to 80°C, add the carbon fiber to the cellulose suspension, stir, and perform ultrasonic stirring for 3 minutes to disperse the carbon fiber. In this step, the length of the carbon fiber is 4 mm, and the power of the ultrasonic stirring is 500W.
[0025] Embodiment 2: A method for high-concentration and stable dispersion of carbon fibers, comprising the following steps:
[0026] Step 1, preparing an alkaline solution with a concentration of 0.75 mol / L, and adding alkali lignin to the alkaline solution to form a mixed solution; wherein the concentration of the alkali lignin in the mixed solution is 1.5 wt%;
[0027] Step 2, heating the mixed solution to 65° C., and then adding 0.3 wt % urea to the mixed solution to obtain a dispersion;
[0028] Step 3: Raise the temperature to 80°C, add the carbon fiber to the cellulose suspension, stir, and perform ultrasonic stirring for 2 minutes to disperse the carbon fiber. In this step, the length of the carbon fiber is 6 mm, and the power of the ultrasonic stirring is 500W.
[0029] Embodiment 3: A method for high-concentration stable dispersion of carbon fibers, comprising the following steps:
[0030] Step 1, preparing an alkaline solution with a concentration of 1 mol / L, and adding alkali lignin to the alkaline solution to form a mixed solution; wherein the concentration of the alkali lignin in the mixed solution is 2 wt%;
[0031] Step 2, heating the mixed solution to 70° C., and then adding 0.5 wt % urea to the mixed solution to obtain a dispersion;
[0032] Step 3: Raise the temperature to 85°C, add the carbon fiber to the cellulose suspension, stir, and perform ultrasonic stirring for 2 minutes to disperse the carbon fiber. In this step, the length of the carbon fiber is 8 mm, and the power of the ultrasonic stirring is 500W.
[0033] Embodiment 4: A method for high-concentration stable dispersion of carbon fibers, comprising the following steps:
[0034] Step 1, preparing an alkaline solution with a concentration of 0.75 mol / L, and adding alkali lignin to the alkaline solution to form a mixed solution; wherein the concentration of the alkali lignin in the mixed solution is 2 wt%;
[0035] Step 2, heating the mixed solution to 60° C., and then adding 0.5 wt % urea to the mixed solution to obtain a dispersion;
[0036] Step 3: Raise the temperature to 100° C., add the carbon fiber to the cellulose suspension, stir, and perform ultrasonic stirring for 1 minute to disperse the carbon fiber. In this step, the length of the carbon fiber is 6 mm, and the power of the ultrasonic stirring is 500W.
[0037] Embodiment 5: A method for high-concentration stable dispersion of carbon fibers, comprising the following steps:
[0038] Step 1, preparing an alkaline solution with a concentration of 1 mol / L, and adding alkali lignin to the alkaline solution to form a mixed solution; wherein the concentration of the alkali lignin in the mixed solution is 1.5 wt%;
[0039] Step 2, heating the mixed solution to 65° C., and then adding urea with a concentration of 1.5 wt % to the mixed solution to obtain a dispersion;
[0040] Step 3: Raise the temperature to 100° C., add the carbon fiber to the cellulose suspension, stir, and perform ultrasonic stirring for 1 minute to disperse the carbon fiber. In this step, the length of the carbon fiber is 6 mm, and the power of the ultrasonic stirring is 500W.
[0041] Embodiment 6: A method for high-concentration stable dispersion of carbon fibers, comprising the following steps:
[0042] Step 1, preparing an alkaline solution with a concentration of 1 mol / L, and adding alkali lignin to the alkaline solution to form a mixed solution; wherein the concentration of the alkali lignin in the mixed solution is 1.5 wt%;
[0043] Step 2, heating the mixed solution to 65° C., and then adding 0.5 wt % urea to the mixed solution to obtain a dispersion;
[0044] Step 3: Raise the temperature to 90°C, add the carbon fiber to the cellulose suspension, stir, and perform ultrasonic stirring for 2 minutes to disperse the carbon fiber. In this step, the length of the carbon fiber is 6 mm, and the power of the ultrasonic stirring is 500W.
[0045] Comparative Example 1: Dispersion of untreated carbon fibers themselves in water.
[0046] Comparative Example 2: Prepare 1 mol / L sodium hydroxide solution, add carbon fiber and stir for 30 minutes.
[0047] Comparative Example 3: Prepare 1 mol / L sodium hydroxide solution, add carbon fiber and carry out ultrasonic stirring for 15 minutes, the power of ultrasonic stirring is 500W.
[0048] The applicant has demonstrated the dispersed carbon fibers in Examples 1-8 and Comparative Examples 1 and 2, as shown in FIG. Figure 1 As shown. Figure 1 It can be seen that the undispersed carbon fiber in comparative example 1 shows agglomeration in the aqueous phase. Comparative example 1 uses conventional alkali solution treatment, and there is still obvious agglomeration, and the dispersion is uneven. Comparative example 2 uses alkali solution and ultrasonic treatment. Although the dispersibility is greatly improved compared with comparative example 2, the ultrasonic time is long, the noise is large, and re-agglomeration is easy to occur after ultrasound. The carbon fiber dispersion shown in Examples 1-6 of the present invention is greatly improved compared with Comparative Examples 1-3, and the carbon fiber is evenly dispersed. Among them, the preferred parameters of Example 6 achieve the best dispersion effect.
[0049] Furthermore, papermaking was carried out with the dispersed carbon fibers in Examples 3-6 and Comparative Example 2. The preparation of the wet paper web is to filter the carbon fibers in each group of suspensions, evenly disperse them into two portions, add 1g APAM to each portion, add 800mL of 80°C hot water and 600mL of cold water to each portion to help disperse the carbon fibers, and then put the two portions into a deflaking machine at the same time for deflaking. After deflaking for 15 minutes, 0.7g PVA fiber and 600mL of 80°C hot water are evenly added to the two suspensions, and the deflaking is continued for 5 minutes before being taken out. The two groups are poured into a paper sheet forming machine at the same time for papermaking. Drying after papermaking: First, use filter paper to absorb the moisture on the surface of the carbon fiber paper, then remove the wet paper web and put it into a wire mesh, place it in a flat dryer and dry it for 15 minutes, then take it out, and place it in a flat vulcanizer and hot press for 10 minutes to obtain the carbon fiber paper with the measured data. The uniformity of each group of papermaking is then statistically analyzed, and the structure is as follows: Figure 2 As shown. Figure 2 It can be found that the uniformity of the paper prepared in Examples 3-6 increases steadily. This is because the carbon fiber pretreatment of the present application can increase the surface hydrophilic groups and the surface roughness structure, improve its hydrophilicity, and make the carbon fiber more evenly dispersed in the suspension, thereby increasing the uniformity of the papermade carbon fiber paper.
[0050] Furthermore, the stability index test was conducted on the dispersed carbon fibers in Examples 3-6 and Comparative Example 2, and their stability was measured by a multiple light scattering instrument. During the test, about 20 mL of the dispersed sample was slowly added to a transparent quartz sample bottle, and the prepared sample pool to be tested was gently picked up vertically, adjusted in direction and placed in a turbiscan room at a temperature of 30°C, and the Turbisoft shortcut was double-clicked to test the sample to be tested according to the TurbiscanLab stability analyzer SOP operating procedures. The results are as follows Figure 3 As shown. Figure 3 It can be seen that the methods of Examples 3-6 have a significant promoting effect on reducing the suspension stability index, and the promoting effect is best in Example 6.
[0051] In summary, the present invention first configures an alkaline solution of alkali lignin, then heats it and adds urea to form an alkali lignin-urea alkaline solution system, thereby in this system, the active groups of alkali lignin are used to modify the carbon fibers, thereby increasing the surface hydrophilic groups and the surface roughness structure, and at the same time, under the action of heating and ultrasonic stirring, the viscosity of the alkali lignin-urea alkaline solution system decreases with increasing temperature, thereby increasing the dispersion speed of the carbon fibers, reducing the interaction force between the carbon fibers, and reducing the internal friction between the carbon fibers, thereby achieving rapid dispersion of the carbon fibers under the influence of multiple factors.
Claims
1. A method for high-concentration and stable dispersion of carbon fiber, characterized in that: The steps include: Step 1, preparing an alkaline solution with a concentration of 0.5-1.5 mol / L, and adding alkali lignin to the alkaline solution to form a mixed solution; wherein the concentration of the alkali lignin in the mixed solution is 1-2 wt%; Step 2, heating the mixed solution to 60-70° C., and then adding 0.3-0.8 wt % urea to the mixed solution to obtain a dispersion; Step 3: Raise the temperature to 80-100° C., add the carbon fiber into the cellulose suspension and stir, and perform ultrasonic stirring for 1-3 minutes to disperse the carbon fiber.
2. The method for high-concentration and stable dispersion of carbon fiber according to claim 1, characterized in that: In step 1, the alkaline solution is a sodium hydroxide solution with a concentration of 1 mol / L.
3. The method for high-concentration and stable dispersion of carbon fiber according to claim 1, characterized in that: The concentration of the alkali lignin is 1.5 wt%.
4. The method for high-concentration and stable dispersion of carbon fiber according to claim 1, characterized in that: In step 2, the mixed solution is heated to 65°C.
5. The method for high-concentration and stable dispersion of carbon fiber according to claim 1, characterized in that: In step 2, the concentration of urea is 0.5 wt %.
6. The method for high-concentration and stable dispersion of carbon fiber according to claim 1, characterized in that: In step 3, the temperature of the ultrasonic stirring is 90°C.
7. The method for high-concentration and stable dispersion of carbon fiber according to claim 1, characterized in that: In step 3, the ultrasonic stirring time is 2 minutes.
8. The method for high-concentration and stable dispersion of carbon fiber according to claim 1, characterized in that: In step 3, the power of the ultrasonic stirring is 500W.
9. The method for high-concentration and stable dispersion of carbon fiber according to claim 1, characterized in that: The length of the carbon fiber is 4-8 mm.
Citation Information
Patent Citations
Preparation method of nitrogen-doped lignin-based carbon fiber composite material
CN108103616A
Preparation method of high-uniformity double-layer gradient pore carbon paper base paper
CN115262278A
Short carbon fiber reinforced wood-epoxy resin type paper-based friction plate and preparation method thereof
CN116732818A
Preparation method and application of carbon fiber dispersion liquid
CN118441474A
Preparation method of double-layer carbon-paper base paper with high uniformity and gradient pores
US20240044081A1