Preparation method of transmission electron microscope sample for biomineralization material atomic-scale imaging
By improving the sample preparation method for transmission electron microscopy and employing conductive silver paste and plasma cleaning techniques, the problem of atomic-level imaging of biomineralized materials was solved, achieving high-resolution atomic-level imaging results.
Patent Information
- Application Number
- CN202411040277.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-26
AI Technical Summary
Existing methods are insufficient for atomic-level imaging of biomineralized materials, and conventional preparation methods cannot meet the requirements for high-resolution observation.
By improving the adhesive between the transmission electron microscope sample and the support ring, strictly controlling the carbon spraying parameters, and performing plasma cleaning and electron beam sweeping during sample preparation, the conductivity of the sample and the thinness of the carbon layer are ensured, thus achieving atomic-level imaging.
The prepared biomineralized material samples can be clearly displayed at the atomic level under a transmission electron microscope, reducing mechanical damage and electron beam damage and improving the observation effect.
Smart Images

Figure HDA0004972201330000011 
Figure HDA0004972201330000012 
Figure HDA0004972201330000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of transmission electron microscope sample preparation, in particular to a transmission electron microscope sample preparation method for atomic-level imaging of biomineralized materials. Background Art
[0002] Transmission Electron Microscope (TEM), also known as TEM for short, projects an accelerated and focused electron beam onto a very thin sample. The electrons collide with the atoms in the sample and change direction, thereby producing a three-dimensional angle scattering. The size of the scattering angle is related to the density and thickness of the sample, so it can form images of different brightness. The image is displayed on the imaging device after being magnified and focused. When using a transmission electron microscope, the electron beam passes through the sample for microscopic imaging. Since the penetration ability of the electron beam is relatively weak, the sample used for transmission electron microscopy analysis must be thin enough to allow the electron beam to pass through and to form a stable image under the irradiation of the electron beam.
[0003] At present, the common methods for preparing transmission electron microscope samples include focused ion beam (FIB) micro-nano processing, ion sputtering thinning and ultra-thin sectioning. Focused ion beam micro-nano processing technology is prone to damage to the sample due to ion beam bombardment during the thinning process, especially for brittle materials sensitive to electron beams, this destructive effect will be more significant. Ion sputtering thinning is also prone to burns on the sample surface due to long sputtering time. Ultra-thin sectioning is very easy to introduce mechanical crack damage to brittle materials. Chinese patent application (CN110926898A) discloses a method for preparing transmission electron microscope samples of electron beam sensitive brittle materials, and specifically discloses: preparing thin slice samples; pre-thinning the thin slice samples by water grinding; thinning the thin slice samples after pre-thinning by low-temperature ion sputtering; carbon spraying the surface of the thin slice samples after low-temperature ion sputtering thinning, so that a layer of amorphous carbon film is deposited on the surface of the thin slice samples. It can be seen that thinning by low-temperature ion sputtering reduces the damage to the sample caused by the high-energy ion beam; spraying carbon on the sample surface increases the conductivity of the sample, which is more conducive to the observation of the microscopic morphology of the sample.
[0004] Biomineralized materials mainly refer to materials with mineralization effects synthesized by organisms. In general, biomineralized materials are not conductive and the image is unstable under electron beam observation. To solve this problem, carbon spraying is usually performed on the surface of the sample. The conventional method for preparing transmission electron microscope samples of biomineralized materials is to use AB glue to glue the sample ring, ion thinning, carbon spraying, and then place it in a transmission electron microscope for observation. However, this method is only suitable for observing the morphology of the sample and conducting simple electron diffraction and energy spectrum analysis experiments, and cannot achieve atomic-level imaging of the sample. Summary of the invention
[0005] The purpose of the present invention is to provide a transmission electron microscope sample preparation method for atomic-level imaging of biomineralized materials, so as to solve the problem that the existing methods are difficult to achieve atomic-level imaging of biomineralized materials.
[0006] The present invention is achieved in that:
[0007] The present invention is based on the objective problems that occur in the process of preparing transmission electron microscope samples of conventional biomineralized materials. By improving the bonding adhesive between the transmission electron microscope sample and the support ring, strictly controlling the carbon spraying parameters, and performing plasma cleaning and electron beam cleaning on the sample after carbon spraying, a sample preparation method with good conductivity, a thin carbon layer on the deposited sample, and atomic-level imaging of the biomineralized material sample is provided.
[0008] The method for preparing transmission electron microscope samples for atomic-level imaging of biomineralized materials provided by the present invention specifically comprises the following steps:
[0009] A. Prepare biomineralized material samples;
[0010] B. Pre-thinning the sample by water grinding;
[0011] C. Glue the sample to the molybdenum ring with conductive silver glue;
[0012] D. Single-gun ion thinning of the sample with the sticky ring;
[0013] E. Carry out double-sided carbon spraying treatment on the surface of the sample after ion thinning;
[0014] F. Place the sample on the sample rod and perform plasma cleaning;
[0015] G. Place the sample into a transmission electron microscope for high electron beam current sweeping. High electron beam current sweeping means that the current density is 23.5 to 25.5 pA / cm 2 Electron beam sweeping.
[0016] Preferably, in step B, the water grinding pre-thinning is to grind the sample on 600#, 1000#, 2000#, and 3000# sandpaper in turn with water and turn "8" shape on both sides to prevent the sample from being subjected to different forces and uneven thickness.
[0017] Preferably, in step C, the sample and the molybdenum ring are connected with conductive silver glue to increase the conductivity of the sample.
[0018] Preferably, step D is specifically as follows: put the sample into the ion thinning instrument, set the ion gun angle to 5°, the voltage to 5keV, select the single gun mode, and thin for 1 hour; then set the ion gun angle to 4°, the voltage to 4keV, and the thinning time to 0.5h. After the thinning time reaches 0.5h, observe whether the sample is transparent. If not, thin again for 0.5h until the sample is transparent; finally, set the ion gun angle to 3°, the voltage to 3keV, and purge for 3min. Thinning the sample in single gun mode can reduce beam damage.
[0019] Preferably, the parameters for carbon spraying the sample in step E are set as follows: pulse length 2s, pulse interval 10s, pulse count 3 times, pulse current 35A, exhaust current 5A, exhaust time 5s. After carbon spraying on both sides of the sample, placing it in a transmission electron microscope can reduce the charging effect.
[0020] Preferably, the sample is plasma cleaned in a plasma cleaning machine for 7 seconds, and the sample is cleaned with a large electron beam in a transmission electron microscope for 30 minutes. Plasma cleaning is performed on the sample before entering the transmission electron microscope, and a large electron beam cleaning treatment is performed on the sample after entering the transmission electron microscope, so as to clean the excessively thick carbon layer deposited on the surface of the sample.
[0021] The atomic image of the transmission electron microscope sample of the biomineralized material prepared by the above method is clearly visible under the transmission electron microscope STEM mode.
[0022] The present invention has the following beneficial effects:
[0023] (1) During the specific water-grinding pre-thinning process, manual "8"-shaped double-sided grinding is used to balance the force in all directions of the sample and ensure uniform thickness.
[0024] (2) Conductive silver glue was used to connect the sample and the molybdenum ring, and the biomineralized material sample was carbon-sprayed on both sides to increase the conductivity of the sample.
[0025] (3) Single-gun ion thinning reduces beam damage.
[0026] (4) Before entering the transmission electron microscope, the sample is cleaned with a plasma cleaner. After entering the transmission electron microscope, the sample is cleaned with a large electron beam to remove the excessively thick carbon layer deposited on the surface of the sample, reduce the interference of the carbon layer, and be more conducive to observing the original atomic-level imaging of the biomineralized material. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the HAADF image of the sample prepared in Example 1 of the present invention at ×5M magnification.
[0028] Figure 2 This is the HAADF image of the sample prepared in Example 4 of the present invention at a magnification of ×5M.
[0029] Figure 3 This is the HAADF image of the sample prepared in Example 6 of the present invention at a magnification of ×5M.
[0030] Figure 4 This is a HAADF image of the sample prepared in Example 6 of the present invention, which shows obvious carbon deposition at a magnification of ×120K after the atomic image reduction factor cannot be adjusted at one position for a long time. DETAILED DESCRIPTION
[0031] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. In the following examples, biological aragonite calcium carbonate nacre is used as a sample, and the transmission electron microscope is a JEM-ARM200F cold field emission condenser spherical aberration corrected transmission electron microscope.
[0032] Example 1
[0033] (1) Use pliers to pick up a small piece of sample slightly smaller than 3 mm, and use hot melt adhesive to stick the sample to the grinding table. Then, add water to 600#, 1000#, 2000#, and 3000# sandpaper and grind it in an "8" shape on both sides until the sample thickness is about 30 μm (for example: 29-31 μm), and then remove the sample.
[0034] (2) Use a cotton swab dipped in acetone to wipe off the hot melt adhesive remaining on the surface of the sample, and then clean the sample with deionized water.
[0035] (3) Take two clean toothpicks and dip them in a little glue A and glue B respectively, mix them evenly to form glue AB; apply a little glue AB on a molybdenum ring with an outer diameter of 3mm, pick up the sample with tweezers, place it on the molybdenum ring and press it with tweezers to make the sample stick to the molybdenum ring (the sample size is smaller than the outer diameter of the molybdenum ring and larger than the inner diameter of the molybdenum ring, which is convenient for pasting the sample and observation under a transmission electron microscope). Put the sample stuck on the molybdenum ring on a piece of paper (molybdenum ring at the bottom and sample at the top), put the paper on a heating table, and bake it at 35℃ until the glue is dry.
[0036] (4) Place the sample into the ion thinning instrument, set the ion gun angle to 5°, the voltage to 5keV, the single gun mode, and the thinning time to 1 hour; then set the ion gun angle to 4°, the voltage to 4keV, and check every half an hour whether the sample is thinned (i.e. whether a hole is thinned out). If not, add another half an hour until the sample is thinned; when the sample is thinned, set the ion gun angle to 3°, the voltage to 3keV, and purge for 3 minutes.
[0037] (5) Place the sample treated with ion thinning on a pure white filter membrane, put it into the sample pool of the carbon spraying instrument, take three strands of carbon filaments and twist them into a twist shape, clamp them into the clamp on the lid of the carbon spraying instrument, cover the lid and evacuate, and spray carbon. After the carbon spraying is completed, use tweezers to move the sample. If the color under the filter membrane sample is different from the surrounding color, it means that carbon has been sprayed. After spraying one side, turn it over and place it on a new pure white filter membrane to repeat the carbon spraying steps. When spraying carbon, the pulse length is set to 2s, the pulse interval is set to 10s, the pulse count is 3 times, the pulse current is 35A, the exhaust current is 5A, and the exhaust time is 5s.
[0038] (6) Place the sample in the transmission electron microscope, select a suitable position, switch to STEM mode, and change the probe size from the original 6C to 1C (i.e., under strong light irradiation) at ×20k. Retract all four STEM detectors in the Image Selector, remove both condenser diaphragms, insert the first-level objective diaphragm and the first-level selection diaphragm, and perform beam sweeping (i.e., BeamShower) for 30 minutes. Then switch back to the normal STEM mode, i.e., probe size 6C, insert the detector, add the first-level condenser diaphragm and the second-level condenser diaphragm, remove the objective diaphragm and the selection diaphragm, and adjust the atomic image.
[0039] When the probe size is 6C, the current density is 0.5~2.5pA / cm 2 ; When the probe size is 1C, the current density becomes 23.5~25.5pA / cm 2 The cleaning in this application is the carbon deposit cleaning under the large electron beam current of 1C, and the atomic image is adjusted under the small electron beam current of 6C. The same below.
[0040] The HAADF image of the sample obtained in this example is as follows: Figure 1 As shown, it can be seen that although the atomic image can be called out at this time, it is not very clear. It is speculated that this may be because the beam cleaning time is not enough.
[0041] Example 2
[0042] (1) Use pliers to pick up a small piece of sample slightly smaller than 3 mm, and use hot melt adhesive to stick the sample to the grinding table. Then, add water to 600#, 1000#, 2000#, and 3000# sandpaper and grind them in an "8" shape on both sides until the sample thickness is about 30 μm. Then remove the sample.
[0043] (2) Use a cotton swab dipped in acetone to wipe off the hot melt adhesive remaining on the surface of the sample, and then clean the sample with deionized water.
[0044] (3) Take two clean toothpicks and dip them in a little glue A and glue B respectively, mix them evenly to form glue AB; apply a little glue AB on a molybdenum ring with an outer diameter of 3 mm, pick up the sample with tweezers, place it on the molybdenum ring and press it slightly with tweezers to make the sample stick to the molybdenum ring, then put the sample with a piece of paper on the heating table and bake it at 35℃ until the glue is dry.
[0045] (4) Place the sample into the ion thinning instrument, set the ion gun angle to 5°, the voltage to 5keV, select the single gun mode, and set the thinning time to 1 hour; then set the angle to 4°, the voltage to 4keV, and check the sample every half an hour of thinning to see if it is transparent until the sample is transparent; finally set the angle to 3°, the voltage to 3keV, and purge for 3 minutes.
[0046] (5) Place the sample treated with ion thinning on a pure white filter membrane, put it into the sample pool of the carbon spraying instrument, take three strands of carbon filaments and twist them into a twist shape, clamp them into the clamp on the lid of the carbon spraying instrument, cover the lid and evacuate, and spray carbon. After the carbon spraying is completed, use tweezers to move the sample. If the color under the filter membrane sample is different from the surrounding color, it means that carbon has been sprayed. After spraying one side, turn it over and place it on a new pure white filter membrane to repeat the carbon spraying steps. When spraying carbon, the pulse length is set to 2s, the pulse interval is set to 10s, the pulse count is 3 times, the pulse current is 35A, the exhaust current is 5A, and the exhaust time is 5s.
[0047] (6) Place the sample in the transmission electron microscope, select a suitable position, switch to STEM mode, and at ×20k magnification, change the probe size to 1C. Retract all four STEM detectors on the image selector, remove both condenser diaphragms, insert the first-level objective diaphragm and the first-level selection diaphragm, and perform beam sweeping for 50 minutes. Then switch back to the normal STEM mode, i.e., probe size 6C, insert the detector, add the first-level condenser diaphragm and the second-level condenser diaphragm, remove the objective diaphragm and the selection diaphragm, and adjust the atomic image.
[0048] In this embodiment, when the sample is observed in a transmission electron microscope, it is found that it is not very stable and will drift. In severe cases, the sample will be blown away by the electron beam. This may be because the beam cleaning time is too long and the carbon used for conductivity on the sample is cleaned too cleanly, which in turn causes a large charging effect on the sample.
[0049] Example 3
[0050] (1) Use pliers to pick up a small piece of sample about 3 mm in diameter, stick it to the sample grinding table with hot melt glue, and grind it on both sides with 600#, 1000#, 2000#, and 3000# sandpaper in an "8" shape with water until the sample thickness is about 30μm, then remove the sample.
[0051] (2) Use a cotton swab dipped in acetone to wipe off the hot melt adhesive remaining on the surface of the sample, and then clean the sample with deionized water.
[0052] (3) Take out the conductive silver glue from the refrigerator, hold the molybdenum ring with tweezers and quickly apply the glue on one side of the molybdenum ring, then lay the molybdenum ring flat, put the sample on the glue of the molybdenum ring, press it gently with tweezers, and wait for the glue to dry. The conductive silver glue is Colloidal Silver with product number 16031 of PELCO, the same below.
[0053] (4) Place the sample into the ion thinning instrument, set the ion gun angle to 5°, the voltage to 5keV, select the single gun mode, and set the thinning time to 1 hour; then set the angle to 4°, the voltage to 4keV, and check the sample every half an hour until the sample is thinned; finally, set the angle to 3°, the voltage to 3keV, and purge for 3 minutes.
[0054] (5) Place the sample treated with ion thinning on a pure white filter membrane, put it into the sample pool of the carbon spraying instrument, take three strands of carbon filaments and twist them into a twist shape, clamp them into the clamp on the lid of the carbon spraying instrument, cover the lid and evacuate, and spray carbon. After the carbon spraying is completed, use tweezers to move the sample. If the color under the filter membrane sample is different from the surrounding color, it means that carbon has been sprayed. After spraying one side, turn it over and place it on a new pure white filter membrane to repeat the carbon spraying steps. When spraying carbon, the pulse length is set to 2s, the pulse interval is set to 10s, the pulse count is 3 times, the pulse current is 35A, the exhaust current is 5A, and the exhaust time is 5s.
[0055] (6) Place the sample in the transmission electron microscope, select a suitable position, switch to STEM mode, and at ×20k magnification, change the probe size to 1C. Retract all four STEM detectors on the image selector, remove all condenser diaphragms of different sizes, insert the first-level objective diaphragm and the first-level selection diaphragm, and perform beam sweeping for 50 minutes. Then switch back to the normal STEM mode, i.e., probe size 6C, insert the detector, add the first-level condenser diaphragm and the second-level condenser diaphragm, remove the objective diaphragm and the selection diaphragm, and adjust the atomic image.
[0056] In this embodiment, the adhesive between the sample and the molybdenum ring is changed, and the conductive silver glue also plays a conductive role, which makes up for the problem of less carbon on the sample surface due to the long beam cleaning time, but the atomic image taken is still not very clear.
[0057] Example 4
[0058] (1) Use pliers to pick up a small piece of sample about 3 mm in diameter, stick it to the sample grinding table with hot melt glue, and grind it on both sides with 600#, 1000#, 2000#, and 3000# sandpaper in an "8" shape with water until the sample thickness is about 30μm, then remove the sample.
[0059] (2) Use a cotton swab dipped in acetone to wipe off the hot melt adhesive remaining on the surface of the sample, and then clean the sample with deionized water.
[0060] (3) Take out the conductive silver glue from the refrigerator, hold the molybdenum ring with tweezers and quickly apply the glue to one side of the molybdenum ring. Then lay the molybdenum ring flat, place the sample on the glue on the molybdenum ring, press it gently with tweezers, and wait for the glue to dry.
[0061] (4) Place the sample into the ion thinning instrument, set the ion gun angle to 5°, the voltage to 5keV, select the single gun mode, and set the thinning time to 1 hour; then set the angle to 4°, the voltage to 4keV, and check the sample every half an hour until the sample is thinned; finally, set the angle to 3°, the voltage to 3keV, and purge for 3 minutes.
[0062] (5) Place the sample treated with ion thinning on a pure white filter membrane, put it into the sample pool of the carbon spraying instrument, take three strands of carbon filaments and twist them into a twist shape, clamp them into the clamp on the lid of the carbon spraying instrument, cover the lid and evacuate, and spray carbon. After the carbon spraying is completed, use tweezers to move the sample. If the color under the filter membrane sample is different from the surrounding color, it means that carbon has been sprayed. After spraying one side, turn it over and place it on a new pure white filter membrane to repeat the carbon spraying steps. When spraying carbon, the pulse length is set to 2s, the pulse interval is set to 10s, the pulse count is 3 times, the pulse current is 35A, the exhaust current is 5A, and the exhaust time is 5s.
[0063] (6) Place the carbon-sprayed sample into the sample rod, then insert the sample rod into a plasma cleaner (or plasma cleaning machine), select the STEM cleaning mode and use O2 and Ar to clean the excess carbon deposited on the sample surface, and set the time to 7s.
[0064] (7) After cleaning, insert the sample rod into the transmission electron microscope, select the position, switch to STEM mode, change the probe size to 1C at ×20k, retract the four STEM detectors, remove the condenser diaphragms of different sizes, insert the first-level objective diaphragm and the first-level selection diaphragm, and perform beam sweeping for 30 minutes. Then switch back to the normal STEM mode, that is, the probe size is 6C, insert the detector, add the first-level condenser diaphragm and the second-level condenser diaphragm, remove the objective diaphragm and the selection diaphragm, and adjust the atomic image.
[0065] Considering that direct irradiation with strong light in the transmission electron microscope and long electron beam cleaning time may be bad for the sample and may cause electron irradiation damage, in this embodiment, after the sample is carbon-sprayed, a plasma cleaner is used to perform a simple carbon deposit cleaning treatment on the sample, and then the sample is put into the transmission electron microscope for large electron beam cleaning. The cleaning only takes 30 minutes, and the atomic image can be easily called out at this time. The results are as follows Figure 2 As shown, the atomic image of the sample in STEM mode is clear.
[0066] Example 5
[0067] (1) Use pliers to pick up a small piece of sample about 3 mm in diameter, stick it to the sample grinding table with hot melt glue, and grind it on both sides with 600#, 1000#, 2000#, and 3000# sandpaper in an "8" shape with water until the sample thickness is about 30μm, then remove the sample.
[0068] (2) Use a cotton swab dipped in acetone to wipe off the hot melt adhesive remaining on the surface of the sample, and then clean the sample with deionized water.
[0069] (3) Take two clean toothpicks and dip them into a little glue A and glue B respectively, mix them evenly to form glue AB; apply a little glue AB on a molybdenum ring with an outer diameter of 3 mm, pick up the sample with tweezers, place it on the molybdenum ring and press it slightly with tweezers, then put the sample with the ring on a heating table with a piece of paper as a cushion, and bake it at 35℃ until the glue is dry.
[0070] (4) Place the sample into the ion thinning instrument, set the ion gun angle to 5°, the voltage to 5keV, select the single gun mode, and set the thinning time to 1 hour; then set the angle to 4°, the voltage to 4keV, and check the sample every half an hour until the sample is thinned; finally, set the angle to 3°, the voltage to 3keV, and purge for 3 minutes.
[0071] (5) Place the sample treated with ion thinning on a pure white filter membrane, put it into the sample pool of the carbon spraying instrument, take three strands of carbon filaments and twist them into a twist shape, clamp them into the clamp on the lid of the carbon spraying instrument, cover the lid and evacuate, and spray carbon. After the carbon spraying is completed, use tweezers to move the sample. If the color under the filter membrane sample is different from the surrounding color, it means that carbon has been sprayed. After spraying one side, turn it over and place it on a new pure white filter membrane to repeat the carbon spraying steps. When spraying carbon, the pulse length is set to 2s, the pulse interval is set to 10s, the pulse count is 3 times, the pulse current is 35A, the exhaust current is 5A, and the exhaust time is 5s.
[0072] (6) Place the carbon-sprayed sample into the sample rod, then insert the sample rod into the plasma cleaner, select the STEM cleaning mode and use O2 and Ar to clean the excess carbon deposited on the sample surface, and set the time to 7s.
[0073] (7) Place the sample into a transmission electron microscope and adjust the atomic image in STEM mode.
[0074] The sample obtained in this embodiment has serious carbon deposition and the atomic image cannot be adjusted.
[0075] Example 6
[0076] (1) Use pliers to pick up a small piece of sample about 3 mm in diameter, stick it to the sample grinding table with hot melt glue, and grind it on both sides with 600#, 1000#, 2000#, and 3000# sandpaper in an "8" shape with water until the sample thickness is about 30μm, then remove the sample.
[0077] (2) Use a cotton swab dipped in acetone to wipe off the hot melt adhesive remaining on the surface of the sample, and then clean the sample with deionized water.
[0078] (3) Take two clean toothpicks and dip them into a little glue A and glue B respectively, mix them evenly to form glue AB; apply a little glue AB on a molybdenum ring with an outer diameter of 3 mm, pick up the sample with tweezers, place it on the molybdenum ring and press it slightly with tweezers, then put the sample with the ring on a heating table with a piece of paper as a cushion, and bake it at 35℃ until the glue is dry.
[0079] (4) Place the sample into the ion thinning instrument, set the ion gun angle to 5°, the voltage to 5keV, select the single gun mode, and set the thinning time to 1 hour; then set the angle to 4°, the voltage to 4keV, and check the sample every half an hour until the sample is thinned; finally, set the angle to 3°, the voltage to 3keV, and purge for 3 minutes.
[0080] (5) Place the sample treated with ion thinning on a pure white filter membrane, put it into the sample pool of the carbon spraying instrument, take three strands of carbon filaments and twist them into a twist shape, clamp them into the clamp on the lid of the carbon spraying instrument, cover the lid and evacuate, and spray carbon. After the carbon spraying is completed, use tweezers to move the sample. If the color under the filter membrane sample is different from the surrounding color, it means that carbon has been sprayed. After spraying one side, turn it over and place it on a new pure white filter membrane to repeat the carbon spraying steps. When spraying carbon, the pulse length is set to 2s, the pulse interval is set to 10s, the pulse count is 3 times, the pulse current is 35A, the exhaust current is 5A, and the exhaust time is 5s.
[0081] (6) Place the sample into a transmission electron microscope and adjust the atomic image in STEM mode.
[0082] The results are as follows Figure 3 As shown. At this time, the white part is seriously carbonized, and the atomic image cannot be obtained by adjusting the same magnification downward, and no useful information can be obtained.
[0083] In the transmission electron microscope sample of the biomineralized material prepared in Example 6, when adjusting the atomic image in the STEM mode, it cannot be adjusted for a long time. After reducing the magnification and changing the observation position of the sample, it is found that the area where the atomic image has just been adjusted is brighter than the rest, such as Figure 4As shown. The reason is that the light for adjusting the atomic image in the STEM mode is a strong electron beam, which will excite the organic molecular groups such as carbon or carbon hydrogen atoms sprayed on the sample surface, and fall back to the sample surface, causing organic molecular contamination on the sample surface, which interferes greatly with the atomic image of the original biomineralized material sample. In Example 4, after the thicker carbon layer sprayed on the sample surface is plasma cleaned, the light beam in the transmission electron microscope is adjusted to the strongest, and the organic molecular groups such as carbon deposited on the sample surface can be directly swept into the lens barrel instead of falling back on the sample surface, further making the carbon layer on the sample surface thinner and cleaner, which is of great significance for adjusting the atomic image of the sample. In order to prevent the electron beam in the electron microscope from sweeping too much and sweeping all the carbon, conductive silver glue is used instead of AB glue. When the electron beam is hit, it will be dispersed through the conductive silver glue, thereby reducing the charge accumulation (i.e., the charging effect), and finally a transmission electron microscope sample suitable for observing the atomic image of biomineralized materials is prepared.
[0084] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing transmission electron microscope samples for atomic-level imaging of biomineralized materials, characterized in that: The steps include: A. Prepare biomineralized material samples; B. Pre-thinning the sample by water grinding; C. Glue the sample to the molybdenum ring with conductive silver glue; D. Single-gun ion thinning of the sample with the sticky ring; E. Carry out double-sided carbon spraying treatment on the surface of the sample after ion thinning; F. Place the sample on the sample rod and perform plasma cleaning; G. Place the sample into a transmission electron microscope for high electron beam current sweeping. High electron beam current sweeping means that the current density is 23.5 to 25.5 pA / cm 2 Electron beam sweeping.
2. The method for preparing transmission electron microscope samples for atomic-level imaging of biomineralized materials according to claim 1, characterized in that: In step G, the sample is swept with a large electron beam in the transmission electron microscope for 30 minutes.
3. The method for preparing transmission electron microscope samples for atomic-level imaging of biomineralized materials according to claim 1, characterized in that: In step F, the sample is plasma cleaned for 7 seconds.
4. The method for preparing transmission electron microscope samples for atomic-level imaging of biomineralized materials according to claim 1, characterized in that: The parameters for carbon spraying on the sample in step E are set as follows: pulse length 2 s, pulse interval 10 s, pulse count 3 times, pulse current 35 A, exhaust current 5 A, and exhaust time 5 s.
5. The method for preparing transmission electron microscope samples for atomic-level imaging of biomineralized materials according to claim 1, characterized in that: Step D is specifically as follows: place the sample into the ion thinning instrument, set the ion gun angle to 5°, the voltage to 5 keV, select the single gun mode, and thin for 1 hour; then set the ion gun angle to 4°, the voltage to 4 keV, and the thinning time to 0.5 hour. After the thinning time reaches 0.5 hour, observe whether the sample is transparent. If not, thin again for 0.5 hour until the sample is transparent; finally, set the ion gun angle to 3°, the voltage to 3 keV, and purge for 3 minutes.
6. The method for preparing transmission electron microscope samples for atomic-level imaging of biomineralized materials according to claim 1, characterized in that: The specific method of water grinding pre-thinning in step B is as follows: the sample is polished on 600#, 1000#, 2000#, and 3000# sandpaper in turn with water in an "8" shape on both sides until the sample thickness is 30±1μm, the sample is removed, and cleaned with acetone and deionized water.
Citation Information
Patent Citations
Preparation method of electron beam sensitive brittle material transmission electron microscope sample
CN110926898A