Preparation method and device of ethanol gas-sensitive detection sensor based on bimetallic oxide semiconductor
The bimetal oxide is synthesized by hydrothermal method and used for the preparation of ethanol sensors, which solves the problems of low detection sensitivity and high detection limit in the prior art, and realizes high sensitivity detection and remote monitoring of low-concentration ethanol gases, which is suitable for large-scale Mass production.
Patent Information
- Application Number
- CN202411120530.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
Existing semiconductor gas sensors have low sensitivity in ethanol detection and high detection limit, making it difficult to achieve accurate and rapid detection in complex environments, especially in low concentrations of ethanol gases.
Hydrothermal method is used to synthesize bimetallic oxides (such as NiFeOx) with different metal proportions, improve the sensitivity of the sensor by regulating the proportion of metal elements, and use it for the preparation of ethanol sensors, combine the structural design of ceramic tubes and gold electrodes, and combine heating. Coil and data acquisition communication circuit to realize remote monitoring and early warning.
It realizes high sensitivity detection for low-concentration ethanol gases, shortens detection time, reduces the lower detection limit, and has good selectivity and anti-interference ability in complex environments, which is suitable for large-scale production.
Smart Images

Figure CN119023738A_ABST
Abstract
Description
Technical field:
[0001] The invention belongs to the technical field of semiconductor gas sensors, and relates to a method for preparing an ethanol detection sensor based on a bimetallic oxide and an application method of the ethanol sensor manufactured based on the bimetallic oxide. Background technology:
[0002] When ethanol gas is inhaled, it will cause harm to the human body, mainly manifested as an inhibitory effect on the central nervous system. Due to its own flammable characteristics, the detection of ethanol gas has important safety application significance in production and life. Long-term exposure to high concentrations of ethanol can cause irritation symptoms of the nasal and eye mucosa. At the same time, it also has important applications in the fields of drunk driving detection and medical testing. Therefore, it is of great significance to develop ethanol sensors with high sensitivity, good selectivity and low detection limit.
[0003] In the field of semiconductor gas sensing, researchers have been continuously deepening their research on improving the sensitivity of oxide semiconductor sensors, reducing the detection limit and optimizing working conditions. In particular, the development of nanoscience and technology has provided a good opportunity to improve sensor performance. Studies have shown that the recognition function, conversion function and sensitive body utilization rate of gas-sensitive materials determine the sensitivity of semiconductor sensors. Many studies have shown that the performance of sensors can be effectively improved by improving the structure and increasing the contact area.
[0004] Through remote wireless monitoring, accurate detection and rapid alarm of ethanol gas can be achieved, which is of great significance in the fields of ethanol production and processing, food transportation and storage, and medical care. Summary of the invention:
[0005] The purpose of the present invention is to provide a bimetallic oxide (NiFe, CuFe, ZnFe, CoFe, etc.) with good gas sensing performance and to make an ethanol sensor based on it. x Take the example of a sensor. By adjusting the ratio of different metal elements in the material, the sensitivity of the sensor is improved and the detection limit is reduced. When it is connected to the detection system, when it is in the ethanol detection scene, detection warning is realized through wireless or wired transmission.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] In the first step, 11-13 mmol Ni(NO 3 ) 2 6H 2 O and Fe(NO 3 ) 3 9H 2 O according to different ratios of Ni and Fe, 15-40mmol (about 1.44g) NH4 F and 85-90 mmol (about 5.16 g) CO(NH 2 ) 2 Dissolve in 30 mL of deionized water;
[0008] The second step is hydrothermal reaction at 110-130°C for 11-14h;
[0009] The third step is to pour the reaction solution into a centrifuge tube, add appropriate amount of ethanol and water into the centrifuge tube, centrifuge at 7000-9000 rpm, take out the centrifuge tube, pour out the supernatant, and dry the obtained sample in a vacuum drying oven.
[0010] The fourth step is to take an appropriate amount of the prepared material and calcine it in a muffle furnace, heating it from room temperature to 320-360°C at a heating rate of 1-3°C per minute, calcine it for 2-3.5h, and then cool it down to room temperature at the same rate;
[0011] After the above steps, the material of the present invention is obtained.
[0012] The preparation method of the bimetallic oxide-based ethanol sensor of the present invention comprises the following steps:
[0013] (1) Grind the calcined material into fine particles, take 40-60 mg of the material and mix it with about 500 μL of anhydrous ethanol, and ultrasonically disperse it for about 5-10 minutes to form a slurry coating;
[0014] (2) Dip the coating and evenly apply it on the surface of the ceramic tube substrate and the gold electrodes wound on the ceramic tube in parallel with each other. The thickness of the sensitive material is about 13 to 30 μm.
[0015] (3) placing the coated ceramic tube in a crucible and aging it in a muffle furnace at 250-300° C. for about 10-14 hours;
[0016] (4) Then, a nickel-chromium alloy heating coil (50 to 60 turns) with a resistance value of about 20 to 40 Ω is passed through the ceramic tube, and the current passing through the heating coil is controlled to provide a suitable operating temperature for the sensor. Finally, the four platinum wires of the sensor and the two ends of the nickel-chromium alloy heating coil are welded to the sensor base;
[0017] (5) The prepared sensor is connected to a detection circuit with data acquisition and communication to realize remote monitoring and early warning of ethanol concentration, thereby obtaining the sensor of the present invention.
[0018] The NiFeO-based x Bimetallic oxide ethanol sensors have the following advantages:
[0019] 1. Bimetallic oxide NiFeO can be synthesized using a simple hydrothermal method x , the synthesis method is simple and easy with low cost;
[0020] 2. By adjusting the ratio of different metal elements, the sensitivity to ethanol is improved, the time required for ethanol detection is greatly shortened, and it can work in a gas atmosphere with a lower concentration (300ppb), which has broad application prospects;
[0021] 3. Use semiconductor tube sensors sold on the market, which have simple device technology, small size and are suitable for mass production. Description of the drawings:
[0022] Figure 1 : Scanning electron microscope photos of the samples of Comparative Example, Example 1, Example 2 and Example 3.
[0023] Figure 2 : XRD of the sample of Example 1.
[0024] Figure 3 : TEM scanning image of Example 2.
[0025] Figure 4 : Relationship between sensitivity and operating temperature of the comparative example, example 1, example 2 and example 2 sample in 20ppm ethanol gas atmosphere.
[0026] Figure 5 : Sensitivity changes of Example 2 at the optimal operating temperature and in ethanol gas of different concentrations.
[0027] Figure 6 : Example 2 is a comparison chart of the sensitivity to various different gases in a 20ppm gas atmosphere.
[0028] Figure 7 : Schematic diagram of the sensor transmitting through wireless devices to achieve remote monitoring and alarm.
[0029] Figure 8 : Schematic diagram of the sensor.
[0030] Figure 1 The following are scanning electron microscope photos of the sensitive materials of the comparative example and each embodiment (a, b, c, d).
[0031] Figure 2 This is the X-ray diffraction pattern of Example 2.
[0032] Figure 3The response of Example 2 in different concentrations of ethanol gas. The three protrusions in the partial enlarged image correspond to 0.3ppm, 0.5ppm and 1ppm ethanol gas concentrations. The sensor has a significant response in lower concentrations of ethanol gas, and the lowest measurable detection limit is about 0.3ppm. The sensitivity (Rg / Ra) is above 50 at 200ppm.
[0033] Figure 4 This is an image of Example 2 under a scanning tunneling microscope. A relatively clear layered structure can be seen, and the interplanar spacing of the corresponding crystal planes is about 0.24 nm.
[0034] Figure 5 The responses of the comparative example, example 1, example 2 and example 3 to ethanol gas with a concentration of about 20 ppm at different temperatures are shown. The three examples obtained the best response at 250° C. Among them, example 2 achieved the best level among all samples.
[0035] Figure 6 The response of Example 2 in various gases is shown in Figure 2, and the corresponding gas concentration is 20 ppm and the temperature is 250° C. This reflects that the sensor has good selectivity and enhanced anti-interference ability in complex environments. Specific implementation method:
[0036] Comparative Example:
[0037] Preparation of NiFeO with different ratios by hydrothermal method x Bimetallic oxide is used to manufacture a semiconductor ethanol gas sensor, and the specific production process is as follows:
[0038] In the first step, 11-13 mmol Ni(NO 3 ) 2 6H 2 O and Fe(NO 3 ) 3 9H 2 O in a ratio of 1:1 between Ni and Fe, 15-40 mmol (about 1.44 g) NH 4 F and 85-90 mmol (about 5.16 g) CO(NH 2 ) 2 Dissolve in 30 mL of deionized water;
[0039] The second step is hydrothermal reaction at 110-130°C for 11-14h;
[0040] The third step is to pour the reaction solution into a centrifuge tube, add appropriate amount of ethanol and water into the centrifuge tube, centrifuge at 7000-9000 rpm, take out the centrifuge tube, pour out the supernatant, and dry the obtained sample in a vacuum drying oven.
[0041] The fourth step is to take an appropriate amount of the prepared material and calcine it in a muffle furnace, heating it from room temperature to 320-360°C at a heating rate of 1-3°C per minute, calcine it for 2-3.5h, and then cool it down to room temperature at the same rate;
[0042] After the above steps, the material of the present invention is obtained.
[0043] The preparation method of the bimetallic oxide-based ethanol sensor of the present invention comprises the following steps:
[0044] (1) Grind the calcined material into fine particles, take 40-60 mg of the material and mix it with about 500 μL of anhydrous ethanol, and ultrasonically disperse it for about 5-10 minutes to form a slurry coating;
[0045] (2) Dip the coating and evenly apply it on the surface of the ceramic tube substrate and the gold electrodes wound on the ceramic tube in parallel with each other. The thickness of the sensitive material is about 13 to 30 μm.
[0046] (3) placing the coated ceramic tube in a crucible and aging it in a muffle furnace at 250-300° C. for about 10-14 hours;
[0047] (4) Then, a nickel-chromium alloy heating coil (50 to 60 turns) with a resistance value of about 20 to 40 Ω is passed through the ceramic tube, and the current passing through the heating coil is controlled to provide a suitable operating temperature for the sensor. Finally, the four platinum wires of the sensor and the two ends of the nickel-chromium alloy heating coil are welded to the sensor base;
[0048] (5) The prepared sensor is connected to a detection circuit with data acquisition and communication to achieve remote monitoring or early warning of ethanol concentration, thereby obtaining the sensor of the present invention.
[0049] Embodiment 1:
[0050] In the first step, 11-13 mmol Ni(NO 3 ) 2 6H 2 O and Fe(NO 3 ) 3 9H 2 O in a ratio of 2:1 between Ni and Fe, 15-40 mmol (about 1.44 g) NH 4 F and 85-90 mmol (about 5.16 g) CO(NH 2 ) 2Dissolve in 30 mL of deionized water;
[0051] The second step is hydrothermal reaction at 110-130°C for 11-14h;
[0052] The third step is to pour the reaction solution into a centrifuge tube, add appropriate amount of ethanol and water into the centrifuge tube, centrifuge at 7000-9000 rpm, take out the centrifuge tube, pour out the supernatant, and dry the obtained sample in a vacuum drying oven.
[0053] The fourth step is to take an appropriate amount of the prepared material and calcine it in a muffle furnace, heating it from room temperature to 320-360°C at a heating rate of 1-3°C per minute, calcine it for 2-3.5h, and then cool it down to room temperature at the same rate;
[0054] After the above steps, the material of the present invention is obtained.
[0055] The preparation method of the bimetallic oxide-based ethanol sensor of the present invention comprises the following steps:
[0056] (1) Grind the calcined material into fine particles, take 40-60 mg of the material and mix it with about 500 μL of anhydrous ethanol, and ultrasonically disperse it for about 5-10 minutes to form a slurry coating;
[0057] (2) Dip the coating and evenly apply it on the surface of the ceramic tube substrate and the gold electrodes wound on the ceramic tube in parallel with each other. The thickness of the sensitive material is about 13 to 30 μm.
[0058] (3) placing the coated ceramic tube in a crucible and aging it in a muffle furnace at 250-300° C. for about 10-14 hours;
[0059] (4) Then, a nickel-chromium alloy heating coil (50 to 60 turns) with a resistance value of about 20 to 40 Ω is passed through the ceramic tube, and the current passing through the heating coil is controlled to provide a suitable operating temperature for the sensor. Finally, the four platinum wires of the sensor and the two ends of the nickel-chromium alloy heating coil are welded to the sensor base;
[0060] (5) The prepared sensor is connected to a detection circuit with data acquisition and communication to achieve remote monitoring or early warning of ethanol concentration, thereby obtaining the sensor of the present invention.
[0061] Embodiment 2:
[0062] In the first step, 11-13 mmol Ni(NO 3 ) 2 6H 2 O and Fe(NO 3 ) 3 9H 2O in a ratio of 3:1 between Ni and Fe, 15-40 mmol (about 1.44 g) NH 4 F and 85-90 mmol (about 5.16 g) CO(NH 2 ) 2 Dissolve in 30 mL of deionized water;
[0063] The second step is hydrothermal reaction at 110-130°C for 11-14h;
[0064] The third step is to pour the reaction solution into a centrifuge tube, add appropriate amount of ethanol and water into the centrifuge tube, centrifuge at 7000-9000 rpm, take out the centrifuge tube, pour out the supernatant, and dry the obtained sample in a vacuum drying oven.
[0065] The fourth step is to take an appropriate amount of the prepared material and calcine it in a muffle furnace, heating it from room temperature to 320-360°C at a heating rate of 1-3°C per minute, calcine it for 2-3.5h, and then cool it down to room temperature at the same rate;
[0066] After the above steps, the material of the present invention is obtained.
[0067] The preparation method of the bimetallic oxide-based ethanol sensor of the present invention comprises the following steps:
[0068] (1) Grind the calcined material into fine particles, take 40-60 mg of the material and mix it with about 500 μL of anhydrous ethanol, and ultrasonically disperse it for about 5-10 minutes to form a slurry coating;
[0069] (2) Dip the coating and evenly apply it on the surface of the ceramic tube substrate and the gold electrodes wound on the ceramic tube in parallel with each other. The thickness of the sensitive material is about 13 to 30 μm.
[0070] (3) placing the coated ceramic tube in a crucible and aging it in a muffle furnace at 250-300° C. for about 10-14 hours;
[0071] (4) Then, a nickel-chromium alloy heating coil (50 to 60 turns) with a resistance value of about 20 to 40 Ω is passed through the ceramic tube, and the current passing through the heating coil is controlled to provide a suitable operating temperature for the sensor. Finally, the four platinum wires of the sensor and the two ends of the nickel-chromium alloy heating coil are welded to the sensor base;
[0072] (5) The prepared sensor is connected to a detection circuit with data acquisition and communication to achieve remote monitoring or early warning of ethanol concentration, thereby obtaining the sensor of the present invention.
[0073] Embodiment 3:
[0074] In the first step, 11-13 mmol Ni(NO3 ) 2 6H 2 O and Fe(NO 3 ) 3 9H 2 O in a ratio of 4:1 between Ni and Fe, 15-40 mmol (about 1.44 g) NH 4 F and 85-90 mmol (about 5.16 g) CO(NH 2 ) 2 Dissolve in 30 mL of deionized water;
[0075] The second step is hydrothermal reaction at 110-130°C for 11-14h;
[0076] The third step is to pour the reaction solution into a centrifuge tube, add appropriate amount of ethanol and water into the centrifuge tube, centrifuge at 7000-9000 rpm, take out the centrifuge tube, pour out the supernatant, and dry the obtained sample in a vacuum drying oven.
[0077] The fourth step is to take an appropriate amount of the prepared material and calcine it in a muffle furnace, heating it from room temperature to 320-360°C at a heating rate of 1-3°C per minute, calcine it for 2-3.5h, and then cool it down to room temperature at the same rate;
[0078] After the above steps, the material of the present invention is obtained.
[0079] The preparation method of the bimetallic oxide-based ethanol sensor of the present invention comprises the following steps:
[0080] (1) Grind the calcined material into fine particles, take 40-60 mg of the material and mix it with about 500 μL of anhydrous ethanol, and ultrasonically disperse it for about 5-10 minutes to form a slurry coating;
[0081] (2) Dip the coating and evenly apply it on the surface of the ceramic tube substrate and the gold electrodes wound on the ceramic tube in parallel with each other. The thickness of the sensitive material is about 13 to 30 μm.
[0082] (3) placing the coated ceramic tube in a crucible and aging it in a muffle furnace at 250-300° C. for about 10-14 hours;
[0083] (4) Then, a nickel-chromium alloy heating coil (50 to 60 turns) with a resistance value of about 20 to 40 Ω is passed through the ceramic tube, and the current passing through the heating coil is controlled to provide a suitable operating temperature for the sensor. Finally, the four platinum wires of the sensor and the two ends of the nickel-chromium alloy heating coil are welded to the sensor base;
[0084] (5) The prepared sensor is connected to a detection circuit with data acquisition and communication to achieve remote monitoring or early warning of ethanol concentration, thereby obtaining the sensor of the present invention.
Claims
1. A preparation method and device of a bimetallic oxide semiconductor ethanol gas-sensitive detection sensor (taking NiFe as an example). It is characterized by: It consists of a sensitive material coated on a ceramic tube substrate with gold electrodes wound parallel to each other at both ends, a nickel-chromium heating wire passing through the ceramic tube, a fixed base and a sensor signal conversion and acquisition system. The sensitive material is NiFeOx bimetallic oxide, which is prepared by the following steps: S1: Dissolve 11-13 mmol Ni(NO3)2·6H2O and Fe(NO3)3·9H2O in different ratios of Ni and Fe, NH4F and CO(NH2)2 in 30 mL of deionized water; S2: hydrothermal reaction at a certain temperature; S3: Pour the reaction solution into a centrifuge tube, add appropriate amount of ethanol and water into the centrifuge tube, centrifuge at 7000-9000 rpm, take out the centrifuge tube, discard the supernatant, and dry the obtained sample in a vacuum drying oven. S4: After heating and calcining, the material of the present invention is obtained.
2. The method for preparing a NiFeOx bimetallic oxide according to claim 1, characterized in that: In the step S1, the amounts of NH4F and CO(NH2)2 used are 15-40 mmol (about 1.44 g) and 85-90 mmol (about 5.16 g).
3. A NiFeO according to claim 1 x A method for preparing a bimetallic oxide, characterized in that: In step S1, the amount of deionized water used is 30 ml.
4. A NiFeO according to claim 1 x A method for preparing a bimetallic oxide, characterized in that: In step S2, the temperature of the hydrothermal reaction is 110-130° C. and the reaction time is 11-13 hours.
5. A NiFeO according to claim 1 x A method for preparing a bimetallic oxide, characterized in that: In step S3, the sample is placed in a vacuum drying chamber at 80° C. for 3 to 5 hours.
6. An ethanol sensor based on NiFeOx material according to claim 1. The manufacturing steps are as follows: S1: Take a small amount of material and grind it into fine particles in a grinding mortar. Take a small amount of material and mix it with an appropriate amount of anhydrous ethanol, and ultrasonically disperse it to form a slurry coating. Dip the coating and evenly apply it on the surface of the ceramic tube substrate and the gold electrodes wound on the ceramic tube in parallel. The thickness of the sensitive material is about 13 to 30 microns; S2: The coated ceramic tube is aged in a muffle furnace at 250-300°C, and then a nickel-chromium alloy heating coil is passed through the ceramic tube. Four platinum wires of the sensor and both ends of the nickel-chromium alloy heating coil are welded to a fixed base of the sensor. The prepared sensor is connected to a detection circuit with data acquisition and communication to realize remote monitoring or early warning of ethanol concentration, thereby obtaining the sensor of the present invention.
7. A NiFeO-based compound according to claims 1-7 x Ethanol detection devices for sensitive materials are used in environmental testing, drunk driving, grain storage and shipping, etc.
8. An ethanol sensor and a detection device thereof, comprising the ethanol sensor according to any one of claims 1 to 7.