Coaxial nano material based on single-walled carbon nanotubes and conductive slurry thereof

By modifying the processing of single-wall carbon nanotubes and forming a three-dimensional conductive network structure, and using specific compounds to prepare conductive paste, the aggregation problem of single-wall carbon nanotubes is solved, and its conductive and dispersive properties are significantly improved. It is applied to composite materials and In electronic devices.

CN119028627AInactive Publication Date: 2024-11-26CHANGZHOU HEXAGON NANOTECHNOLOGY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411226127.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Single-walled carbon nanotubes often show agglomeration during synthesis and application, resulting in uneven distribution in matrix materials and affecting their performance, especially in composite materials and electronic devices.

Method used

Pretreated single-wall carbon nanotubes were generated by the reaction of polyvinylpyrrolidone, zinc nitrate hexahydrate and 2-methylimidazole by modification treatment on single-wall carbon nanotubes, and nickel-rich metal phosphides were grown through hydrothermal reactions. , forming a three-dimensional conductive network structure; at the same time, dispersants are prepared using compounds such as 4,4'-dihydroxybenzophenone, epoxychlorohydrin and α-cyclodextrin to form a conductive paste through grinding to enhance the carbon nanotubes Dispersing and conducting properties.

Benefits of technology

It significantly improves the conductivity and dispersion properties of single-wall carbon nanotubes, improves its uniformity and stability in composite materials and electronic devices, and improves the mechanical and electrical conductivity of the materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of conductive paste, in particular to a coaxial nanomaterial based on a single-walled carbon nanotube and conductive paste thereof. The preparation method comprises the following steps: adding polyvinylpyrrolidone, modified single-walled carbon nanotubes, zinc nitrate hexahydrate and 2-methylimidazole to obtain a mixed solution; carrying out vacuum drying and high-temperature calcination on the mixed solution to obtain the pretreated single-walled carbon nanotube. And dissolving the pretreated single-walled carbon nanotube, nickel nitrate hexahydrate and red phosphorus in deionized water, mixing, and carrying out hydrothermal reaction to obtain the coaxial nano material based on the single-walled carbon nanotube. 4, 4 '-dihydroxybenzophenone, epoxy chloropropane, alpha-cyclodextrin and sodium hydroxide are added, and a dispersing agent is obtained; and mixing the dispersing agent, the coaxial nano material and deionized water, and fully grinding to obtain the conductive paste. The conductive paste prepared by the invention has good conductivity and dispersion performance, so that the conductive paste has a wide application prospect in the technical field of conductive paste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of conductive pastes, in particular to a coaxial nano material based on single-walled carbon nanotubes and a conductive paste thereof. Background Art

[0002] Single-walled carbon nanotube (SWCNT) is a special coaxial nanomaterial. Its structure is composed of a single layer of carbon atoms arranged in a tubular form. This structure makes SWCNT exhibit unique physical and chemical properties at the nanoscale. Therefore, single-walled carbon nanotubes have significant value in modern science and technology and industry, as follows: First, the excellent electrical conductivity and highly controllable electronic properties of single-walled carbon nanotubes make them an ideal material for the new generation of nanoelectronic devices. Single-walled carbon nanotubes with coaxial structures can effectively reduce current density and reduce thermal effects in devices, thereby improving the working stability and life of devices. In addition, coaxial nanomaterials of single-walled carbon nanotubes have also shown broad application prospects in the field of composite materials. Its high strength and lightweight characteristics make it a key component of high-performance composite materials. These composite materials can not only significantly improve the strength and toughness of structural materials, but also reduce the total weight of the materials. This is of great significance in the fields of aerospace, automobile manufacturing and construction engineering.

[0003] However, single-walled carbon nanotubes often show agglomeration during the synthesis and application process, which will lead to uneven distribution in the matrix material, thus affecting its final performance. Therefore, it is necessary to improve the dispersion performance of SWCNT to ensure its uniform distribution in the composite material and avoid the performance degradation caused by agglomeration. This uniform distribution is crucial for the mechanical properties, electrical conductivity and thermal conductivity of the composite material. In addition, single-walled carbon nanotubes are also widely used in electronic devices due to their excellent electrical conductivity. In high-performance electronic devices, by improving the high electrical conductivity of SWCNT, the resistance can be reduced and the working efficiency and response speed of the device can be improved. In summary, improving the dispersion and electrical conductivity of single-walled carbon nanotubes can not only improve their uniformity and stability in composite materials, but also significantly improve their performance in electronic devices, energy storage devices and other high-tech applications.

[0004] In order to overcome the defects of the prior art, the present invention provides a coaxial nanomaterial based on single-walled carbon nanotubes and a conductive paste thereof. Summary of the invention

[0005] The object of the present invention is to provide a coaxial nanomaterial based on single-walled carbon nanotubes and a conductive paste thereof to solve the problems in the prior art.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A coaxial nanomaterial based on single-walled carbon nanotubes comprises the following steps:

[0008] Step 1: dissolving polyvinyl pyrrolidone in methanol, adding modified single-walled carbon nanotubes, stirring for 30-50 minutes to obtain a suspension; adding zinc nitrate hexahydrate solution to the suspension, stirring for 1-2 hours, adding 2-methylimidazole solution and continuing to stir for 1-2 hours to obtain a mixed solution; vacuum drying the mixed solution at 60-70° C. for 10-12 hours to obtain a mixed powder; then heating the mixed powder to 800-850° C. and calcining for 3-4 hours to obtain pretreated single-walled carbon nanotubes;

[0009] Step 2: dissolving the pretreated single-walled carbon nanotubes in deionized water, and ultrasonically dispersing for 40-60 minutes to obtain dispersion 1; adding nickel nitrate hexahydrate and red phosphorus to the deionized water, and stirring for 40-50 minutes to obtain dispersion 2; quickly mixing dispersion 1 and dispersion 2, and hydrothermally reacting at 180-200° C. for 15-18 hours. After the reaction is completed, cooling, washing, and drying are performed to obtain a coaxial nanomaterial based on single-walled carbon nanotubes.

[0010] More optimally, in step 1, zinc nitrate hexahydrate is dissolved in methanol to obtain a zinc nitrate hexahydrate solution; and 2-methylimidazole is dissolved in methanol to obtain a 2-methylimidazole solution.

[0011] More optimally, in step 1, the reaction mass ratio of polyvinyl pyrrolidone, modified single-walled carbon nanotubes, zinc nitrate hexahydrate and 2-methylimidazole is 1.2:(3-4):15:16.

[0012] More optimally, the preparation process of modified single-walled carbon nanotubes is as follows: adding single-walled carbon nanotubes to 15-20wt% nitric acid solution, ultrasonically dispersing for 50-60 minutes, stirring and reacting at 120-130°C for 3.5-4.0 hours, vacuum filtering, washing, and vacuum drying after the reaction to obtain modified single-walled carbon nanotubes.

[0013] More optimally, in step 2, the reaction mass ratio of pretreated single-walled carbon nanotubes, nickel nitrate hexahydrate and red phosphorus is (0.4-0.5):0.15:0.6.

[0014] A conductive paste prepared based on the coaxial nanomaterial comprises the following steps: S1: 4,4'-dihydroxybenzophenone and epichlorohydrin are mixed, and then a catalyst triphenylphosphine is added, and a ring-opening reaction is carried out at 120-130°C for 3-6h. After the reaction is completed, the intermediate product is obtained by rotary evaporation, extraction, and drying; α-cyclodextrin is added to a 0.02-0.03 mg / L sodium hydroxide solution, and the mixture is stirred and heated to 50-60°C, and then the intermediate product is added to continue the reaction at a constant temperature for 45-50h. After the reaction is completed, the dispersion agent is obtained by cooling, filtering, rotary evaporation, reflux extraction, rotary evaporation again, and vacuum drying;

[0015] S2: Add the dispersant to deionized water, stir thoroughly for 30-40 minutes, then add the coaxial nanomaterial, grind to an average particle size of 7-8 μm, and obtain a conductive slurry.

[0016] More optimally, in step S1, the contents of the dispersant components are: by mass, 64-68 parts of 4,4'-dihydroxybenzophenone, 55-60 parts of epichlorohydrin, 0.4-0.5 parts of triphenylphosphine, 10-12 parts of α-cyclodextrin, and 0.0004-0.0006 parts of sodium hydroxide.

[0017] More optimally, in step S2, the contents of the components of the conductive paste are: by mass fraction, 8-12% coaxial nanomaterial, 2-3% dispersant, and the remainder is deionized water.

[0018] Beneficial effects of the present invention:

[0019] The present invention is characterized in that, in step 1, a mixed solution is obtained by adding polyvinyl pyrrolidone, modified single-walled carbon nanotubes, zinc nitrate hexahydrate and 2-methylimidazole; the mixed solution is then vacuum dried and calcined at high temperature to obtain pretreated single-walled carbon nanotubes. In this step, a three-dimensional conductive network structure with high porosity is obtained by welding the modified single-walled carbon nanotubes using a metal organic framework MOF material through an in-situ growth method. Through the treatment of this step, the conductive performance of the single-walled carbon nanotubes can be improved.

[0020] The present invention is characterized in that in step 2, pretreated single-walled carbon nanotubes, nickel nitrate hexahydrate and red phosphorus are dissolved in deionized water, mixed and subjected to hydrothermal reaction to obtain a coaxial nanomaterial based on single-walled carbon nanotubes. In this step, nickel-rich metal phosphide is grown on the surface of the pretreated single-walled carbon nanotubes through hydrothermal reaction, and the substance has good electrical properties. Therefore, by further growing a conductive material on the surface of the pretreated single-walled carbon nanotubes with a three-dimensional conductive network structure, the synergistic effect of the three conductive materials can be promoted, thereby significantly improving the conductive properties of the single-walled carbon nanotubes, and obtaining a coaxial nanomaterial with excellent conductive properties.

[0021] The feature of the present invention is that when preparing the conductive paste, 4,4'-dihydroxybenzophenone, epichlorohydrin, α-cyclodextrin and sodium hydroxide are added to obtain a dispersant; and then a dispersant, a coaxial nanomaterial and deionized water are added, and the conductive paste is obtained after sufficient grinding. In this step, 4,4'-dihydroxybenzophenone and epichlorohydrin are subjected to a ring-opening reaction to prepare an intermediate product, and the intermediate product has a large benzene ring and a chlorine group. Furthermore, the intermediate product is subjected to a substitution reaction with α-cyclodextrin and sodium hydroxide to prepare a dispersant, and the dispersant has a large number of cyclic structures that can interact with carbon nanotubes through hydrogen bonds and the like to form a coating layer, and the coating layer can reduce the agglomeration phenomenon between carbon nanotubes and enhance the dispersion of carbon nanotubes. In summary, the conductive paste prepared by the present invention has good conductivity and dispersion properties, and therefore has broad application prospects in the field of conductive paste technology. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Source of raw materials:

[0024] Single-walled carbon nanotubes, provided by Guangzhou Hongwu Material Technology Co., Ltd., have a diameter of 2 nm; polyvinyl pyrrolidone, provided by Hubei Xinghengye Technology Co., Ltd., is industrial grade and has a molecular weight of 111; one portion is 1 g by mass.

[0025] Example 1: Step 1: adding single-walled carbon nanotubes to a 20wt% nitric acid solution, ultrasonically dispersing for 60 minutes, stirring and reacting at 130°C for 4.0 hours, vacuum filtering, washing, and vacuum drying after the reaction to obtain modified single-walled carbon nanotubes;

[0026] Dissolve polyvinyl pyrrolidone in methanol, add modified single-walled carbon nanotubes, and stir for 50 minutes to obtain a suspension; dissolve zinc nitrate hexahydrate in methanol to obtain a zinc nitrate hexahydrate solution; dissolve 2-methylimidazole in methanol to obtain a 2-methylimidazole solution; add the zinc nitrate hexahydrate solution to the suspension, stir for 2 hours, then add the 2-methylimidazole solution and continue stirring for 2 hours to obtain a mixed solution;

[0027] The mixed solution was vacuum dried at 70°C for 12 hours to obtain a mixed powder; the mixed powder was then heated to 850°C and calcined for 4 hours to obtain pretreated single-walled carbon nanotubes; wherein the reaction mass ratio of polyvinyl pyrrolidone, modified single-walled carbon nanotubes, zinc nitrate hexahydrate and 2-methylimidazole was 1.2:4:15:16;

[0028] Step 2: dissolving the pretreated single-walled carbon nanotubes in deionized water, and ultrasonically dispersing for 60 minutes to obtain dispersion 1; adding nickel nitrate hexahydrate and red phosphorus to the deionized water, and stirring for 50 minutes to obtain dispersion 2; quickly mixing dispersion 1 and dispersion 2, and hydrothermally reacting at 200° C. for 18 hours, cooling, washing, and drying after the reaction to obtain a coaxial nanomaterial based on single-walled carbon nanotubes; wherein the reaction mass ratio of the pretreated single-walled carbon nanotubes, nickel nitrate hexahydrate, and red phosphorus is 0.5:0.15:0.6;

[0029] Step 3: Mix 64g of 4,4'-dihydroxybenzophenone and 55g of epichlorohydrin, add 0.4g of catalyst triphenylphosphine, and carry out ring-opening reaction at 130°C for 6h. After the reaction, perform rotary evaporation, extraction, and drying to obtain an intermediate product; then add 10g of α-cyclodextrin to 0.03mg / L sodium hydroxide solution (0.0004g of sodium hydroxide), stir well and heat to 60°C, then add the intermediate product and continue to react at a constant temperature for 50h. After the reaction, cool, filter, rotary evaporate, reflux extraction, rotary evaporate again, and vacuum dry to obtain a dispersant;

[0030] Step 4: Add 2% dispersant to 88% deionized water by mass fraction, stir thoroughly for 40 minutes, add 10% coaxial nanomaterial, grind to an average particle size of 8 μm, and obtain a conductive slurry.

[0031] Example 2: Step 1: adding single-walled carbon nanotubes to a 20wt% nitric acid solution, ultrasonically dispersing for 55 minutes, stirring and reacting at 125°C for 3.7 hours, vacuum filtering, washing, and vacuum drying after the reaction to obtain modified single-walled carbon nanotubes;

[0032] Dissolve polyvinyl pyrrolidone in methanol, add modified single-walled carbon nanotubes, and stir for 40 minutes to obtain a suspension; dissolve zinc nitrate hexahydrate in methanol to obtain a zinc nitrate hexahydrate solution; dissolve 2-methylimidazole in methanol to obtain a 2-methylimidazole solution; add the zinc nitrate hexahydrate solution to the suspension, stir for 1.5 hours, then add the 2-methylimidazole solution and continue stirring for 1.5 hours to obtain a mixed solution;

[0033] The mixed solution was vacuum dried at 65°C for 11 hours to obtain a mixed powder; the mixed powder was then heated to 825°C and calcined for 3.5 hours to obtain pretreated single-walled carbon nanotubes; wherein the reaction mass ratio of polyvinyl pyrrolidone, modified single-walled carbon nanotubes, zinc nitrate hexahydrate and 2-methylimidazole was 1.2:4:15:16;

[0034] Step 2: dissolving the pretreated single-walled carbon nanotubes in deionized water, and ultrasonically dispersing for 50 minutes to obtain dispersion 1; adding nickel nitrate hexahydrate and red phosphorus to the deionized water, and stirring for 45 minutes to obtain dispersion 2; quickly mixing dispersion 1 and dispersion 2, and hydrothermally reacting at 190° C. for 17 hours, and cooling, washing, and drying after the reaction to obtain a coaxial nanomaterial based on single-walled carbon nanotubes; wherein the reaction mass ratio of the pretreated single-walled carbon nanotubes, nickel nitrate hexahydrate, and red phosphorus is 0.5:0.15:0.6;

[0035] Step 3: Mix 64g of 4,4'-dihydroxybenzophenone and 55g of epichlorohydrin, add 0.4g of catalyst triphenylphosphine, carry out ring-opening reaction at 125°C for 5h, and after the reaction, rotary evaporation, extraction, and drying are performed to obtain an intermediate product; then add 10g of α-cyclodextrin to 0.025mg / L sodium hydroxide solution (0.0004g of sodium hydroxide), stir well and heat to 55°C, then add the intermediate product and continue to react at a constant temperature for 47h. After the reaction, cool, filter, rotary evaporate, reflux extraction, rotary evaporate again, and vacuum dry to obtain a dispersant;

[0036] Step 4: Add 2% dispersant to 88% deionized water by mass fraction, stir thoroughly for 35 minutes, add 10% coaxial nanomaterial, grind to an average particle size of 8 μm, and obtain a conductive slurry.

[0037] Example 3: Step 1: adding single-walled carbon nanotubes to a 20wt% nitric acid solution, ultrasonically dispersing for 50 minutes, stirring and reacting at 120°C for 3.5 hours, vacuum filtering, washing, and vacuum drying after the reaction to obtain modified single-walled carbon nanotubes;

[0038] Dissolve polyvinyl pyrrolidone in methanol, add modified single-walled carbon nanotubes, and stir for 30 minutes to obtain a suspension; dissolve zinc nitrate hexahydrate in methanol to obtain a zinc nitrate hexahydrate solution; dissolve 2-methylimidazole in methanol to obtain a 2-methylimidazole solution; add the zinc nitrate hexahydrate solution to the suspension, stir for 1 hour, then add the 2-methylimidazole solution and continue stirring for 1 hour to obtain a mixed solution;

[0039] The mixed solution was vacuum dried at 60°C for 10 hours to obtain a mixed powder; the mixed powder was then heated to 800°C and calcined for 3 hours to obtain pretreated single-walled carbon nanotubes; wherein the reaction mass ratio of polyvinyl pyrrolidone, modified single-walled carbon nanotubes, zinc nitrate hexahydrate and 2-methylimidazole was 1.2:4:15:16;

[0040] Step 2: dissolving the pretreated single-walled carbon nanotubes in deionized water, and ultrasonically dispersing for 40 minutes to obtain dispersion 1; adding nickel nitrate hexahydrate and red phosphorus to the deionized water, and stirring for 40 minutes to obtain dispersion 2; quickly mixing dispersion 1 and dispersion 2, and hydrothermally reacting at 180° C. for 15 hours, and cooling, washing, and drying after the reaction to obtain a coaxial nanomaterial based on single-walled carbon nanotubes; wherein the reaction mass ratio of the pretreated single-walled carbon nanotubes, nickel nitrate hexahydrate, and red phosphorus is 0.5:0.15:0.6;

[0041] Step 3: Mix 64g of 4,4'-dihydroxybenzophenone and 55g of epichlorohydrin, add 0.4g of catalyst triphenylphosphine, and carry out ring-opening reaction at 120°C for 3h. After the reaction, rotary evaporation, extraction, and drying are performed to obtain an intermediate product; then 10g of α-cyclodextrin is added to 0.02mg / L sodium hydroxide solution (0.0004g of sodium hydroxide), stirred thoroughly and heated to 50°C, and then the intermediate product is added to continue the reaction at a constant temperature for 45h. After the reaction, cooling, filtering, rotary evaporation, reflux extraction, rotary evaporation again, and vacuum drying are performed to obtain a dispersant;

[0042] Step 4: Add 2% dispersant to 88% deionized water by mass fraction, stir thoroughly for 30 minutes, add 10% coaxial nanomaterial, grind to an average particle size of 8 μm, and obtain a conductive slurry.

[0043] Comparative Example 1: excluding step 2, the rest is the same as Example 1, and the specific steps are as follows: Step 1: adding single-walled carbon nanotubes to 20wt% nitric acid solution, ultrasonically dispersing for 60min, and then stirring at 130°C for 4.0h. After the reaction is completed, vacuum filtration, washing, and vacuum drying are obtained to obtain modified single-walled carbon nanotubes;

[0044] Dissolve polyvinyl pyrrolidone in methanol, add modified single-walled carbon nanotubes, and stir for 50 minutes to obtain a suspension; dissolve zinc nitrate hexahydrate in methanol to obtain a zinc nitrate hexahydrate solution; dissolve 2-methylimidazole in methanol to obtain a 2-methylimidazole solution; add the zinc nitrate hexahydrate solution to the suspension, stir for 2 hours, then add the 2-methylimidazole solution and continue stirring for 2 hours to obtain a mixed solution;

[0045] The mixed solution was vacuum dried at 70°C for 12 hours to obtain a mixed powder; the mixed powder was then heated to 850°C and calcined for 4 hours to obtain pretreated single-walled carbon nanotubes; wherein the reaction mass ratio of polyvinyl pyrrolidone, modified single-walled carbon nanotubes, zinc nitrate hexahydrate and 2-methylimidazole was 1.2:4:15:16;

[0046] Step 2: 64g of 4,4'-dihydroxybenzophenone and 55g of epichlorohydrin are mixed, and then 0.4g of catalyst triphenylphosphine is added, and a ring-opening reaction is carried out at 130°C for 6h. After the reaction is completed, the intermediate product is obtained by rotary evaporation, extraction, and drying; then 10g of α-cyclodextrin is added to 0.03mg / L sodium hydroxide solution (0.0004g of sodium hydroxide), and the mixture is stirred and heated to 60°C, and then the intermediate product is added and the reaction is continued at a constant temperature for 50h. After the reaction is completed, the dispersant is obtained by cooling, filtering, rotary evaporation, reflux extraction, rotary evaporation, and vacuum drying;

[0047] Step 3: Add 2% dispersant to 88% deionized water by mass, stir thoroughly for 40 minutes, add 10% pretreated single-walled carbon nanotubes, grind to an average particle size of 8 μm, and obtain a conductive slurry.

[0048] Comparative Example 2: The coaxial nanomaterial prepared by the present invention is replaced with single-walled carbon nanotubes, and the rest is the same as Example 1, and the specific steps are as follows: Step 1: 64g of 4,4'-dihydroxybenzophenone and 55g of epichlorohydrin are mixed, and then 0.4g of catalyst triphenylphosphine is added, and a ring-opening reaction is carried out at 130°C for 6h. After the reaction is completed, it is subjected to rotary evaporation, extraction, and drying to obtain an intermediate product; then 10g of α-cyclodextrin is added to 0.03mg / L sodium hydroxide solution (0.0004g of sodium hydroxide), fully stirred and heated to 60°C, and then the intermediate product is added to continue the reaction at a constant temperature for 50h. After the reaction is completed, it is cooled, filtered, rotary evaporated, refluxed, extracted, rotary evaporated again, and vacuum dried to obtain a dispersant;

[0049] Step 2: By mass fraction, add 2% dispersant to 88% deionized water, stir thoroughly for 40 minutes, then add 10% single-walled carbon nanotubes, grind to an average particle size of 8 μm, and obtain a conductive slurry.

[0050] Comparative Example 3: The dispersant prepared by the present invention is replaced with sodium dodecyl sulfate, and the rest is the same as Example 1, and the specific steps are as follows: Step 1: Add the single-walled carbon nanotubes to a 20wt% nitric acid solution, ultrasonically disperse for 60 minutes, and then stir and react at 130°C for 4.0 hours. After the reaction is completed, vacuum filter, wash, and vacuum dry to obtain modified single-walled carbon nanotubes;

[0051] Dissolve polyvinyl pyrrolidone in methanol, add modified single-walled carbon nanotubes, and stir for 50 minutes to obtain a suspension; dissolve zinc nitrate hexahydrate in methanol to obtain a zinc nitrate hexahydrate solution; dissolve 2-methylimidazole in methanol to obtain a 2-methylimidazole solution; add the zinc nitrate hexahydrate solution to the suspension, stir for 2 hours, then add the 2-methylimidazole solution and continue stirring for 2 hours to obtain a mixed solution;

[0052] The mixed solution was vacuum dried at 70°C for 12 hours to obtain a mixed powder; the mixed powder was then heated to 850°C and calcined for 4 hours to obtain pretreated single-walled carbon nanotubes; wherein the reaction mass ratio of polyvinyl pyrrolidone, modified single-walled carbon nanotubes, zinc nitrate hexahydrate and 2-methylimidazole was 1.2:4:15:16;

[0053] Step 2: dissolving the pretreated single-walled carbon nanotubes in deionized water, and ultrasonically dispersing for 60 minutes to obtain dispersion 1; adding nickel nitrate hexahydrate and red phosphorus to the deionized water, and stirring for 50 minutes to obtain dispersion 2; quickly mixing dispersion 1 and dispersion 2, and hydrothermally reacting at 200° C. for 18 hours, cooling, washing, and drying after the reaction to obtain a coaxial nanomaterial based on single-walled carbon nanotubes; wherein the reaction mass ratio of the pretreated single-walled carbon nanotubes, nickel nitrate hexahydrate, and red phosphorus is 0.5:0.15:0.6;

[0054] Step 3: By mass fraction, add 2% sodium dodecyl sulfate to 88% deionized water, stir thoroughly for 40 minutes, then add 10% coaxial nanomaterials, grind to an average particle size of 8 μm, and obtain a conductive paste.

[0055] Detection test:

[0056] Conductivity test: The conductive paste prepared by the present invention was coated on a polyimide insulating substrate with a 300 μm scraper and dried at 100° C. for 60 min. The obtained carbon film was subjected to roller pressing as a sample, and the conductivity of the film was tested by using a four-probe method.

[0057] Slurry stability test: The conductive slurry prepared by the present invention was placed in a room temperature environment for 3 months, and the conductivity of the carbon film after coating was tested to obtain the conductivity of the carbon film coated with the conductive slurry after 3 months of placement. The stability of the slurry was evaluated by calculating the percentage of the change in the initial conductivity relative to the initial conductivity. The results are shown in the following table:

[0058] Conductivity / (S / cm) Conductivity change rate / (%) Example 1 580 4.5 Example 2 574 4.6 Example 3 571 4.8 Comparative Example 1 533 4.6 Comparative Example 2 460 4.6 Comparative Example 3 573 5.6

[0059] Conclusion: The dosage of Examples 1 to 3 remains unchanged, and only some reaction parameters are modified. From the experimental data, it can be seen that there is no obvious fluctuation in the performance of the samples.

[0060] Comparative Example 1: Step 2 is removed, and the rest is the same as Example 1. It can be seen from the experimental data that compared with Example 1, the conductivity is reduced to 533S / cm. The reason is analyzed as follows: after removing step 2, compared with Example 1, the surface of the pretreated single-walled carbon nanotube lacks the conductive material nickel-rich metal phosphide, and only the MOF material and the single-walled carbon nanotubes work synergistically. Therefore, compared with Example 1, the conductive performance will decrease and the conductivity will decrease.

[0061] Comparative Example 2: The coaxial nanomaterial prepared by the present invention is replaced by single-walled carbon nanotubes, and the rest is the same as Example 1. It can be seen from the experimental data that compared with Example 1, the conductivity is reduced to 460S / cm. The reason is analyzed as follows: after the coaxial nanomaterial prepared by the present invention is replaced by single-walled carbon nanotubes, compared with Example 1, the conductive material MOF material and nickel-rich metal phosphide are lacking, so the conductive performance will decrease compared with Example 1, and the conductivity is reduced.

[0062] Comparative Example 3: The dispersant prepared by the present invention is replaced by sodium dodecyl sulfate, and the rest is the same as Example 1. It can be seen from the experimental data that compared with Example 1, the conductivity change rate increases by 5.6%. The reason is analyzed as follows: the dispersant prepared by the present invention has a large number of ring structures that can interact with carbon nanotubes through hydrogen bonds and the like to form a coating layer, thereby effectively improving the agglomeration phenomenon and enhancing the stability of the conductive slurry. Therefore, after replacing it with sodium dodecyl sulfate, the stability of the conductive slurry decreases and the conductivity change rate increases.

[0063] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.

[0064] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a coaxial nanomaterial based on single-walled carbon nanotubes, characterized in that: The following steps are involved: Step 1: dissolve polyvinyl pyrrolidone in methanol, add modified single-walled carbon nanotubes, and stir thoroughly for 30-50 minutes to obtain a suspension; Adding zinc nitrate hexahydrate solution to the suspension, stirring for 1-2 hours, then adding 2-methylimidazole solution and continuing stirring for 1-2 hours to obtain a mixed solution; vacuum drying the mixed solution at 60-70° C. for 10-12 hours to obtain a mixed powder; then heating the mixed powder to 800-850° C. and calcining for 3-4 hours to obtain pretreated single-walled carbon nanotubes; Step 2: dissolving the pretreated single-walled carbon nanotubes in deionized water, and ultrasonically dispersing for 40-60 minutes to obtain dispersion 1; adding nickel nitrate hexahydrate and red phosphorus to the deionized water, and stirring for 40-50 minutes to obtain dispersion 2; quickly mixing dispersion 1 and dispersion 2, and hydrothermally reacting at 180-200° C. for 15-18 hours. After the reaction is completed, cooling, washing, and drying are performed to obtain a coaxial nanomaterial based on single-walled carbon nanotubes.

2. The method for preparing a coaxial nanomaterial based on single-walled carbon nanotubes according to claim 1, characterized in that: In step 1, zinc nitrate hexahydrate is dissolved in methanol to obtain a zinc nitrate hexahydrate solution; and 2-methylimidazole is dissolved in methanol to obtain a 2-methylimidazole solution.

3. The method for preparing a coaxial nanomaterial based on single-walled carbon nanotubes according to claim 1, characterized in that: In step 1, the reaction mass ratio of polyvinyl pyrrolidone, modified single-walled carbon nanotubes, zinc nitrate hexahydrate and 2-methylimidazole is 1.2:(3-4):15:

16.

4. The method for preparing a coaxial nanomaterial based on single-walled carbon nanotubes according to claim 3, characterized in that: The preparation process of modified single-walled carbon nanotubes is as follows: adding single-walled carbon nanotubes to 15-20wt% nitric acid solution, ultrasonically dispersing for 50-60 minutes, stirring and reacting at 120-130°C for 3.5-4.0 hours, vacuum filtering, washing, and vacuum drying after the reaction to obtain modified single-walled carbon nanotubes.

5. The method for preparing a coaxial nanomaterial based on single-walled carbon nanotubes according to claim 1, characterized in that: In step 2, the reaction mass ratio of the pretreated single-walled carbon nanotubes, nickel nitrate hexahydrate and red phosphorus is (0.4-0.5):0.15:0.

6.

6. A coaxial nanomaterial based on single-walled carbon nanotubes, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 5.

7. A conductive paste prepared based on the coaxial nanomaterial according to claim 6, characterized in that: The following steps are involved: S1: Mix 4,4'-dihydroxybenzophenone and epichlorohydrin, add triphenylphosphine as a catalyst, and carry out a ring-opening reaction at 120-130°C for 3-6 hours. After the reaction, perform rotary evaporation, extraction, and drying to obtain an intermediate product; Then, add α-cyclodextrin to 0.02-0.03 mg / L sodium hydroxide solution, stir thoroughly and heat to 50-60°C, then add the intermediate product and continue to react at constant temperature for 45-50 hours. After the reaction is completed, cool, filter, rotary evaporate, reflux extract, rotary evaporate again, and vacuum dry to obtain a dispersant; S2: Add the dispersant to deionized water, stir thoroughly for 30-40 minutes, then add the coaxial nanomaterial, grind to an average particle size of 7-8 μm, and obtain a conductive slurry.

8. The conductive paste according to claim 7, characterized in that: In step S1, the contents of the dispersant components are as follows: by mass: 64-68 parts of 4,4'-dihydroxybenzophenone, 55-60 parts of epichlorohydrin, 0.4-0.5 parts of triphenylphosphine, 10-12 parts of α-cyclodextrin, and 0.0004-0.0006 parts of sodium hydroxide.

9. The conductive paste according to claim 7, characterized in that: In step S2, the contents of the components of the conductive paste are: by mass fraction, 8-12% of coaxial nanomaterials, 2-3% of dispersant, and the balance is deionized water.

Citation Information

Cited By

  • Enamel material and preparation method thereof

    CN120664779A

  • Enamel material and method for its production

    CN120664779B