Method for preparing Nb3Sn superconducting material through rapid heating and Nb3Sn superconducting material
By adopting two-step heat treatment in the preparation of Nb3Sn superconducting materials, fast heating is used to suppress grain growth and improve critical current density, the performance problem caused by long heat treatment time in the prior art is solved, and the high magnetic field superconducting magnet is realized Performance improvement.
Patent Information
- Application Number
- CN202411181024.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-26
AI Technical Summary
During the preparation of existing Nb3Sn superconducting materials, long-term heat treatment leads to the growth of grains, the grain boundary density decreases, and the critical current density (Jc) is insufficient, which cannot meet the performance requirements of high-magnetic field superconducting magnets.
The heat treatment is carried out by two-step method. During the second heat treatment, the heating is increased at a fast temperature increase rate of 0.5℃/s-3℃/s, which shortens the heat treatment time, inhibits the growth of Nb3Sn grains, and obtains the superconducting phase of fine grains, thereby increasing the criticality. Current density.
It significantly shortens the heat treatment time, inhibits grain growth, improves the magnetic flux pinning force and critical current density of Nb3Sn superconducting materials, and meets the performance requirements of high-magnetic field superconducting magnets.
Smart Images

Figure CN119028656A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of superconducting material preparation and relates to a method for preparing Nb by rapid heating. 3 Sn superconducting material method and Nb 3 Sn superconducting material. Background Art
[0002] Nb 3 Sn has a high upper critical field H c2 (27T, 4.2K) and critical temperature T c (18.3K) is currently the preferred superconducting material for building high magnetic field magnets (above 10T), and has important application prospects in particle accelerators, high energy physics and nuclear fusion devices.
[0003] Nb 3 Sn superconducting materials are usually wound into superconducting magnets in the form of wires and used in various fields. 3 The preparation methods of Sn superconducting wire mainly include bronze method, internal tin method and powder tube method. 3 Sn has a typical A15 phase structure, which is very brittle. Therefore, it is usually necessary to wind the precursor wire into a coil before heat treatment. 3 The formation of Sn superconducting phase usually requires multiple heat treatments on the wire, and the whole process takes hundreds of hours. The long heat treatment makes the production cycle too long, which is not conducive to actual production needs. In addition, the long heat treatment is easy to cause Nb 3 As Sn grains grow, the grain boundary density decreases, which eventually leads to the critical current density (J c ) decreases, and the magnet performance decreases.
[0004] For Nb 3 For high magnetic field superconducting magnets wound with Sn wire, the J c It is an important performance indicator. According to literature reports, the planned Future Circular Collider (FCC) needs to have a high J in order to increase the energy of particle collisions. c The accelerator magnet is used to bend the particle beam. Specifically, the FCC magnet is required to have about 2000A / mm at 4.2K and 15T. 2 J c However, currently Nb 3 Sn conductor J c The level is only up to 1600A / mm 2 -1700A / mm 2 (4.2K@15T).
[0005] Therefore, it is urgent to increase Nb 3Critical current density of Sn. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention aims to provide a method for preparing Nb by rapid heating. 3 Sn superconducting material method and Nb 3 Sn superconducting material. The present invention adopts a two-step method for heat treatment. During the second heat treatment, the temperature is raised at a fast heating rate of 0.5℃ / s-3℃ / s to achieve rapid heating. The rapid heating method can significantly shorten the heat treatment time. Due to the shortened heat treatment time, Nb 3 Sn grain growth is suppressed, and finally Nb with fine grains can be obtained. 3 Sn superconducting phase, thereby improving the magnetic flux pinning force and obtaining a high critical current density (J c ).
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a method for preparing Nb by rapid heating. 3 A method for making Sn superconducting materials, the method comprising:
[0009] (1) mixing single-element Nb powder, single-element Sn powder and single-element Cu powder to obtain a mixed powder;
[0010] (2) pressing the mixed powder to obtain a block product;
[0011] (3) The bulk product is subjected to a first heat treatment and a second heat treatment in sequence to obtain Nb 3 Sn superconducting material;
[0012] The first heat treatment includes a first heating stage, a first heat preservation stage and a first cooling stage which are carried out in sequence; the second heat treatment includes a second heating stage, a second heat preservation stage and a second cooling stage which are carried out in sequence, and the heating rate of the second heating stage is 0.5°C / s-3°C / s, for example, 0.5°C / s, 0.6°C / s, 0.7°C / s, 0.8°C / s, 0.9°C / s, 1°C / s, 1.1°C / s, 1.2°C / s. s, 1.3℃ / s, 1.4℃ / s, 1.5℃ / s, 1.6℃ / s, 1.7℃ / s, 1.8℃ / s, 1.9℃ / s, 2℃ / s, 2.1℃ / s, 2.2℃ / s, 2.3℃ / s, 2.4℃ / s, 2.5℃ / s, 2.6℃ / s, 2.7℃ / s, 2.8℃ / s, 2.9℃ / s or 3℃ / s, but is not limited to the listed values, and other values not listed within the numerical range are equally applicable.
[0013] The present invention provides a method for preparing Nb3 In the method for Sn superconducting material, a two-step method is used for heat treatment, specifically a first heat treatment and a second heat treatment are performed in sequence. During the second heat treatment, the temperature is increased at a fast heating rate of 0.5°C / s-3°C / s to achieve rapid heating. The rapid heating method can significantly shorten the heat treatment time. Due to the shortened heat treatment time, Nb 3 Sn grain growth is suppressed, and finally Nb with fine grains can be obtained. 3 Sn superconducting phase, thereby improving the magnetic flux pinning force, and then obtaining a high critical current density. The preparation process of the method of the present invention is simple and easy to implement, and is suitable for preparing Nb with high critical current density. 3 Sn superconducting wire provides important ideas.
[0014] In the present invention, when the heating rate of the second heat treatment is controlled to be 0.5°C / s-3°C / s, the Nb 3 The critical current density of Sn superconducting material is better.
[0015] Preferably, the average particle size of the single-substance Nb powder in step (1) is 1 μm-8 μm, for example, it can be 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm or 8 μm.
[0016] In the present invention, the single substance Nb powder is used to prepare Nb 3 One of the raw materials of Sn superconducting materials, when the average particle size of single Nb powder is in the range of 1μm-8μm, it is more conducive to the preparation of Nb with higher critical current density. 3 Sn superconducting material.
[0017] Preferably, the average particle sizes of the elemental Sn powder and the elemental Cu powder in step (1) are independently 30 μm-60 μm, for example, 30 μm, 32 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm or 60 μm, etc., but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0018] Preferably, the purity of the elemental Nb powder, elemental Sn powder and elemental Cu powder is independently 99wt.%-99.99wt.%, for example, it can be 99wt.%, 99.10wt.%, 99.50wt.%, 99.90wt.%, 99.95wt.% or 99.99wt.%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0019] Preferably, the molar ratio of the elemental Nb powder, the elemental Sn powder and the elemental Cu powder is 3:1:(1-6), for example, it can be 3:1:1, 3:1:2, 3:1:3, 3:1:4, 3:1:5 or 3:1:6, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] In the present invention, when the addition amount of the single substance Cu powder satisfies the molar ratio of the single substance Nb powder, the single substance Sn powder and the single substance Cu powder is 3:1:(1-6), it is more conducive to preparing Nb with a higher critical current density. 3 Sn superconducting material.
[0021] Preferably, the mixing method in step (1) includes wet grinding.
[0022] Preferably, the solvent used in the wet grinding comprises anhydrous ethanol.
[0023] Preferably, the volume ratio of the total volume of the elemental Nb powder, elemental Sn powder and elemental Cu powder to anhydrous ethanol is 1:(1-2), for example, it can be 1:1, 1:1.5 or 1:2, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] Preferably, the wet grinding time is 30 min-60 min, for example, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] Preferably, the compression molding method in step (2) comprises a powder filling method.
[0026] Preferably, the powder tube filling method comprises:
[0027] (a) providing a stainless steel tube with one end open and the other end closed and a metal tantalum sheet, curling the metal tantalum sheet into a cylindrical shape and placing it in the inner cavity of the stainless steel tube, and making the metal tantalum sheet close to the inner cavity side wall of the stainless steel tube;
[0028] (b) The mixed powder is loaded into the inner cavity of a stainless steel tube, and then a copper column is placed above the mixed powder, and the copper column is cold pressed to close the open end of the stainless steel tube to obtain a block product, wherein the block product includes a Nb-Sn-Cu block and an external coating coated on the surface of the Nb-Sn-Cu block.
[0029] The present invention uses a metal tantalum sheet as a barrier layer material, which is located between the stainless steel tube and the mixed powder. Its function is to prevent the mixed powder from contacting the stainless steel tube and avoiding mutual diffusion between the two.
[0030] In the present invention, the Nb-Sn-Cu block is formed by cold pressing of mixed powder. The external coating body is composed of a stainless steel tube, a metal tantalum sheet and a copper column.
[0031] Preferably, the stainless steel tube is cylindrical in shape.
[0032] Preferably, the height of the stainless steel tube is 20mm-50mm, for example, it can be 20mm, 25mm, 30mm, 35mm, 40mm, 45mm or 50mm; the outer diameter of the stainless steel tube is 20mm-30mm, for example, it can be 20mm, 21mm, 22mm, 23mm, 24mm, 25mm, 26mm, 27mm, 28mm, 29mm or 30mm; the inner diameter of the stainless steel tube is 10%-20% smaller than the outer diameter, for example, it can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0033] Preferably, the size of the metal tantalum sheet is (30-80) mm×(20-30) mm×(20-50) μm, for example, it can be 30 mm×20 mm×20 μm, 40 mm×22 mm×30 μm, 50 mm×24 mm×35 μm, 60 mm×26 mm×40 μm, 70 mm×28 mm×45 mm or 80 mm×30 mm×50 μm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] Preferably, the mass of the mixed powder loaded into the stainless steel tube is 5g-20g, for example, 5g, 8g, 10g, 12g, 14g, 16g, 18g or 20g, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] Preferably, the copper column is cylindrical in shape.
[0036] Preferably, the height of the copper column is 20mm-50mm, for example, it can be 20mm, 25mm, 30mm, 35mm, 40mm, 45mm or 50mm; the diameter of the copper column is 1%-3% smaller than the inner diameter of the stainless steel tube, for example, it can be 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.6%, 2.8% or 3%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] Preferably, the copper column is made of T2 copper or oxygen-free copper.
[0038] Preferably, the cold pressing pressure is 10t-20t, for example, it can be 10t, 11t, 12t, 13t, 14t, 15t, 16t, 17t, 18t, 19t or 20t, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] Preferably, the first heat treatment is performed in a tube furnace.
[0040] Preferably, the atmosphere of the first heat treatment is a protective atmosphere.
[0041] Preferably, the heating rate of the first heating stage is 10°C / h-30°C / h, for example, it can be 10°C / h, 11°C / h, 12°C / h, 13°C / h, 14°C / h, 15°C / h, 16°C / h, 17°C / h, 18°C / h, 19°C / h, 20°C / h, 21°C / h, 22°C / h, 23°C / h, 24°C / h, 25°C / h, 26°C / h, 27°C / h, 28°C / h, 29°C / h or 30°C / h, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0042] Preferably, the insulation temperature of the first insulation stage is 580℃-620℃, for example, it can be 580℃, 585℃, 590℃, 595℃, 599℃, 600℃, 605℃, 610℃, 615℃ or 620℃, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0043] Preferably, the insulation time of the first insulation stage is 30h-60h, for example, it can be 30h, 32h, 35h, 38h, 40h, 42h, 45h, 48h, 50h, 52h, 55h, 58h or 60h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0044] Preferably, the first cooling stage is to cool naturally with the furnace to 25°C-35°C, for example, it can be 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, 31°C, 32°C, 33°C, 34°C or 35°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0045] Preferably, the second heat treatment is performed in an induction heating furnace.
[0046] In the present invention, the first heat treatment is performed in a tubular furnace, the purpose of which is to perform a relatively long sintering heat treatment at a low temperature stage to achieve Cu-Sn homogenization; the second heat treatment is performed in an induction heating furnace, the purpose of which is to perform rapid heating and short-time heat preservation.
[0047] Preferably, the atmosphere of the second heat treatment is a protective atmosphere.
[0048] Preferably, the insulation temperature of the second insulation stage is 950℃-1050℃, for example, it can be 950℃, 980℃, 1000℃, 1020℃ or 1050℃, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0049] Preferably, the insulation time of the second insulation stage is 0s-300s, for example, it can be 0s, 1s, 10s, 20s, 30s, 50s, 60s, 90s, 100s, 120s, 150s, 180s, 200s, 210s, 240s, 250s, 270s, 280s or 300s, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0050] In the present invention, the second heat preservation stage has a heat preservation time of 0s-300s, and the heat preservation time is short, which can shorten the heat treatment time. In the second heat treatment step, the present invention simultaneously performs rapid heating and short-time heat preservation, which can significantly shorten the heat treatment time and effectively inhibit Nb 3 The growth of Sn grains further increases the critical current density.
[0051] Preferably, the second cooling stage is to cool naturally with the furnace to 25°C-35°C, for example, it can be 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, 31°C, 32°C, 33°C, 34°C or 35°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0052] Preferably, in step (3), after the second heat treatment, the outer coating is removed to obtain Nb 3 Sn superconducting material.
[0053] Preferably, the outer covering is removed by cutting.
[0054] As a preferred technical solution of the present invention, the method specifically comprises the following steps:
[0055] (I) adding elemental Nb powder, elemental Sn powder and elemental Cu powder into a mortar in a molar ratio of 3:1:(1-6), adding anhydrous ethanol, and wet grinding in the mortar for 30 min-60 min to obtain a mixed powder; wherein the purity of the elemental Nb powder, elemental Sn powder and elemental Cu powder is independently 99wt.%-99.99wt.%; the average particle size of the elemental Nb powder is 1μm-8μm; the average particle size of the elemental Sn powder and elemental Cu powder is independently 30μm-60μm; the volume ratio of the total volume of the elemental Nb powder, elemental Sn powder and elemental Cu powder to anhydrous ethanol is 1:(1-2);
[0056] (II) providing a stainless steel tube with one end open and the other end closed, the stainless steel tube being cylindrical in shape, the height of the stainless steel tube being 20 mm to 50 mm, the outer diameter being 20 mm to 30 mm, and the inner diameter being 10% to 20% smaller than the outer diameter; and providing a metal tantalum sheet with a size of (30-80) mm × (20-30) mm × (20-50) μm; curling the metal tantalum sheet into a cylindrical shape and placing it in the inner cavity of the stainless steel tube, and making the metal tantalum sheet close to the inner cavity side wall of the stainless steel tube, and then adding 5 g to 20 g of the mixed The mixed powder is loaded into the inner cavity of a stainless steel tube, and a copper column is placed above the mixed powder, and a pressure of 10t-20t is applied to the copper column for cold pressing to close the open end of the stainless steel tube to obtain a block product, wherein the block product includes a Nb-Sn-Cu block and an external coating coated on the surface of the Nb-Sn-Cu block; wherein the shape of the copper column is cylindrical, the height of the copper column is 20mm-50mm, the diameter of the copper column is 1%-3% smaller than the inner diameter of the stainless steel tube, and the material of the copper column is T2 copper or oxygen-free copper;
[0057] (III) placing the block product obtained in step (II) in a tubular furnace and performing a first heat treatment in a flowing argon atmosphere, wherein the specific process of the first heat treatment is: heating to 580°C-620°C at a heating rate of 10°C / h-30°C / h, keeping the temperature for 30h-60h, and then naturally cooling to 25°C-35°C with the furnace; then placing the block product after the first heat treatment in an induction heating furnace and performing a second heat treatment in an argon atmosphere, wherein the specific process of the second heat treatment is: heating to 950°C-1050°C at a heating rate of 0.5°C / s-3°C / s, keeping the temperature for 0s-300s, and then naturally cooling to 25°C-35°C with the furnace; then cutting the block product after the second heat treatment using an electric spark cutting device to remove the external coating to obtain Nb 3 Sn superconducting material.
[0058] In a second aspect, the present invention provides a Nb 3 Sn superconducting material, the Nb 3The Sn superconducting material is prepared by the method described in the first aspect.
[0059] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0060] Compared with the prior art, the present invention has the following beneficial effects:
[0061] The present invention provides a method for preparing Nb 3 In the method for Sn superconducting material, a two-step method is used for heat treatment, specifically a first heat treatment and a second heat treatment are performed in sequence. During the second heat treatment, the temperature is increased at a fast heating rate of 0.5°C / s-3°C / s to achieve rapid heating. The rapid heating method can significantly shorten the heat treatment time. Due to the shortened heat treatment time, Nb 3 Sn grain growth is suppressed, and finally Nb with fine grains can be obtained. 3 Sn superconducting phase, thereby improving the magnetic flux pinning force, and then obtaining a high critical current density. The preparation process of the method of the present invention is simple and easy to implement, and is suitable for preparing Nb with high critical current density. 3 Sn superconducting wire provides important ideas. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 The Nb obtained in Examples 1, 2 and 3 of the present invention 3 XRD pattern of Sn superconducting material.
[0063] Figure 2 The Nb obtained in Examples 1, 2 and 3 of the present invention 3 Critical current density test results of Sn superconducting material.
[0064] Figure 3 Nb obtained in Examples 4, 5 and 6 of the present invention 3 XRD pattern of Sn superconducting material.
[0065] Figure 4 Nb obtained in Example 4 of the present invention 3 SEM image of Sn superconducting material.
[0066] Figure 5 Nb obtained in Example 5 of the present invention 3 SEM image of Sn superconducting material.
[0067] Figure 6 Nb obtained in Example 6 of the present invention 3 SEM image of Sn superconducting material.
[0068] Figure 7 Nb obtained in Example 7 and Example 2 of the present invention 3 Critical current density test results of Sn superconducting material.
[0069] Figure 8 Nb obtained in Example 8 and Example 2 of the present invention 3 Critical current density test results of Sn superconducting material.
[0070] Fig. 9 Nb obtained in Example 9 and Example 2 of the present invention 3 Critical current density test results of Sn superconducting material.
[0071] Fig.10 The Nb obtained in Comparative Example 1 of the present invention 3 SEM image of Sn superconducting material.
[0072] Fig.11 The Nb obtained in Comparative Example 1 and Example 5 of the present invention 3 Critical current density test results of Sn superconducting material.
[0073] Fig.12 The Nb obtained in Comparative Example 2 and Example 2 of the present invention 3 Critical current density test results of Sn superconducting material.
[0074] Fig.13 The Nb obtained in Comparative Example 3 and Example 2 of the present invention 3 Critical current density test results of Sn superconducting material. DETAILED DESCRIPTION
[0075] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0076] Example 1
[0077] This embodiment provides a method for preparing Nb by rapid heating 3 The method for Sn superconducting material comprises the following steps:
[0078] (1) adding elemental Nb powder, elemental Sn powder and elemental Cu powder into a mortar in a molar ratio of 3:1:1, and adding anhydrous ethanol, wherein the volume ratio of the total volume of the elemental Nb powder, elemental Sn powder and elemental Cu powder to the anhydrous ethanol is 1:2, and wet grinding is performed in the mortar for 30 minutes to obtain a mixed powder; wherein the purity of the elemental Nb powder, elemental Sn powder and elemental Cu powder is independently 99.99wt.%; the average particle size of the elemental Nb powder is 3μm; the average particle size of the elemental Sn powder and elemental Cu powder is 45μm;
[0079] (2) providing a stainless steel tube with one end open and the other end closed, the stainless steel tube being cylindrical in shape, the height of the stainless steel tube being 30 mm, the outer diameter being 20 mm, and the inner diameter being 10% smaller than the outer diameter; and providing a metal tantalum sheet with a size of 50 mm×20 mm×30 μm; curling the metal tantalum sheet into a cylindrical shape and placing it in the inner cavity of the stainless steel tube, and making the metal tantalum sheet close to the inner cavity side wall of the stainless steel tube, and then loading 10 g of the mixed powder into the inner cavity of the stainless steel tube, and then placing the copper column in the inner cavity of the stainless steel tube. The copper column is shaped like a cylinder, has a height of 30 mm, has a diameter 1% smaller than the inner diameter of the stainless steel tube, and is made of T2 copper. A pressure of 10 t is then applied to the copper column on a tablet press to perform cold pressing so that the open end of the stainless steel tube is closed to obtain a block product, wherein the block product includes a Nb-Sn-Cu block and an external coating coated on the surface of the Nb-Sn-Cu block, wherein the external coating consists of a stainless steel tube, a metal tantalum sheet, and a copper column;
[0080] (3) placing the block product obtained in step (2) in a tubular furnace and performing a first heat treatment in a flowing argon atmosphere, wherein the specific process of the first heat treatment is: heating to 600°C at a heating rate of 20°C / h, keeping the temperature for 50 hours, and then naturally cooling to 25°C with the furnace; then placing the block product after the first heat treatment in an induction heating furnace and performing a second heat treatment in an argon atmosphere, wherein the specific process of the second heat treatment is: heating to 1000°C at a heating rate of 1°C / s, keeping the temperature for 30 seconds, and then naturally cooling to 25°C with the furnace; then cutting the block product after the second heat treatment with an electric spark cutting machine to remove the external coating to obtain Nb 3 Sn superconducting material.
[0081] Example 2
[0082] The difference between this embodiment and embodiment 1 is that the holding time of the second heat treatment in step (3) is changed to 120 seconds.
[0083] The remaining steps and conditions are the same as those in Example 1.
[0084] Example 3
[0085] The difference between this embodiment and embodiment 1 is that the holding time of the second heat treatment in step (3) is changed to 240s.
[0086] The remaining steps and conditions are the same as those in Example 1.
[0087] Figure 1 The Nb obtained in Example 1, Example 2 and Example 3 is shown. 3 XRD test results of Sn superconducting materials. As shown in the figure, the Nb3 In Sn superconducting materials, Nb 3 Sn was the main phase, and no Nb was detected, which indicated that after rapid heating and short-term heat preservation, almost all Nb participated in the reaction, and Nb reacted with Sn to generate a large amount of target Nb. 3 Sn superconducting phase.
[0088] Critical current density test: The Nb obtained in Example 1, Example 2 and Example 3 3 A 2mm×2mm×2mm cubic block of Sn superconducting material was cut out, and then the hysteresis loop (MH) was measured in the external magnetic field range of 2T-8T at a temperature of 4.2K using a comprehensive physical property measurement system (PPMS). Finally, the critical current density was calculated using the Bean model.
[0089] Figure 2 The Nb obtained in Example 1, Example 2 and Example 3 is shown. 3 The critical current density of Sn superconducting materials (J c ) test results, showing that the Nb of Examples 1-3 3 The critical current density J of Sn superconducting material at 4.2K c (Unit: A / mm 2 ) changes with the magnetic field (unit is T). It can be seen from the figure that Nb 3 Sn superconducting material has a very high critical current density in the entire test magnetic field range. For example, J c They are: 23800A / mm 2 、22000A / mm 2 and 17700A / mm 2 These values are far higher than those of Nb prepared by bronze method. 3 J of Sn wire c .
[0090] Example 4
[0091] This embodiment provides a method for preparing Nb by rapid heating 3 The method for Sn superconducting material comprises the following steps:
[0092] (1) adding elemental Nb powder, elemental Sn powder and elemental Cu powder into a mortar in a molar ratio of 3:1:1, and adding anhydrous ethanol, wherein the volume ratio of the total volume of the elemental Nb powder, elemental Sn powder and elemental Cu powder to the anhydrous ethanol is 1:2, and wet grinding is performed in the mortar for 40 minutes to obtain a mixed powder; wherein the purity of the elemental Nb powder, elemental Sn powder and elemental Cu powder is independently 99.95wt.%; the average particle size of the elemental Nb powder is 5μm; the average particle size of the elemental Sn powder and elemental Cu powder is 50μm;
[0093] (2) providing a stainless steel tube with one end open and the other end closed, the stainless steel tube being cylindrical in shape, the height of the stainless steel tube being 40 mm, the outer diameter being 30 mm, and the inner diameter being 20% smaller than the outer diameter; and providing a metal tantalum sheet with a size of 80 mm×30 mm×30 μm; curling the metal tantalum sheet into a cylindrical shape and placing it in the inner cavity of the stainless steel tube, and making the metal tantalum sheet close to the inner cavity side wall of the stainless steel tube, and then loading 20 g of the mixed powder into the inner cavity of the stainless steel tube, and then placing the copper column in the inner cavity of the stainless steel tube. The copper column is shaped like a cylinder, has a height of 40 mm, has a diameter 3% smaller than the inner diameter of the stainless steel tube, and is made of T2 copper. A pressure of 20 t is then applied to the copper column on a tablet press to perform cold pressing so that the open end of the stainless steel tube is closed to obtain a block product, wherein the block product includes a Nb-Sn-Cu block and an external coating coated on the surface of the Nb-Sn-Cu block, wherein the external coating consists of a stainless steel tube, a metal tantalum sheet, and a copper column;
[0094] (3) placing the block product obtained in step (2) in a tubular furnace and performing a first heat treatment in a flowing argon atmosphere, wherein the specific process of the first heat treatment is: heating to 580°C at a heating rate of 30°C / h, keeping the temperature for 60h, and then naturally cooling to 25°C with the furnace; then placing the block product after the first heat treatment in an induction heating furnace and performing a second heat treatment in an argon atmosphere, wherein the specific process of the second heat treatment is: heating to 1000°C at a heating rate of 1°C / s, keeping the temperature for 60s, and then naturally cooling to 25°C with the furnace; then cutting the block product after the second heat treatment with an electric spark cutting machine to remove the external coating to obtain Nb 3 Sn superconducting material.
[0095] Example 5
[0096] The difference between this embodiment and embodiment 4 is that the molar ratio of elemental Nb powder, elemental Sn powder and elemental Cu powder in step (1) is changed to 3:1:3.
[0097] The remaining steps and conditions are the same as those in Example 4.
[0098] Example 6
[0099] The difference between this embodiment and embodiment 4 is that the molar ratio of elemental Nb powder, elemental Sn powder and elemental Cu powder in step (1) is changed to 3:1:5.
[0100] The remaining steps and conditions are the same as those in Example 4.
[0101] Figure 3 The Nb obtained in Example 4, Example 5 and Example 6 is shown. 3 The XRD test results of Sn superconducting materials show that the Nb 3 In Sn superconducting materials, Nb 3 Sn is the main phase, which shows that even if the initial Cu ratio is increased, Nb is still generated after heat treatment. 3 The target superconducting phase is mainly Sn.
[0102] Figure 4-6 The Nb obtained in Example 4, Example 5 and Example 6 are shown respectively. 3 The SEM microstructure of Sn superconducting material shows that the Nb 3 The SEM microstructure of Sn superconducting materials has a similar composition, where the black is the Cu-Sn matrix, the gray is the residual Nb, and the white is the large distribution of Nb. 3 Sn superconducting phase, which shows that the present invention can form a large amount of target Nb after rapid heating and short-term heat preservation 3 Sn superconducting phase.
[0103] Example 7
[0104] The difference between this embodiment and embodiment 2 is that the molar ratio of elemental Nb powder, elemental Sn powder and elemental Cu powder in step (1) is changed to 3:1:11.5.
[0105] The remaining steps and conditions are the same as those in Example 2.
[0106] The Nb obtained in Example 7 was tested using the test method described above. 3 Critical current density of Sn superconducting material.
[0107] Figure 7 The Nb obtained in Example 7 and Example 2 is shown. 3 The critical current density test results of Sn superconducting materials show that Nb 3 The critical current density J of Sn superconducting material at 4.2K c (Unit: A / mm 2 ) changes with the magnetic field (unit: T). As can be seen from the figure, the Nb obtained in Example 7 3J of Sn superconducting material in the whole tested magnetic field range c The results are significantly lower than those in Example 2, which indicates that even if the rapid heating method proposed in the present invention is adopted, excessive increase in the proportion of initial Cu powder will also lead to Nb 3 J of Sn superconducting materials c Significantly reduced, therefore, the proportion of initial Cu powder needs to be reasonably controlled.
[0108] Example 8
[0109] The difference between this embodiment and embodiment 2 is that the average particle size of the elemental Nb powder in step (1) is changed to 45 μm.
[0110] The remaining steps and conditions are the same as those in Example 2.
[0111] The Nb obtained in Example 8 was tested using the test method described above. 3 Critical current density of Sn superconducting material.
[0112] Figure 8 The Nb obtained in Example 8 and Example 2 is shown. 3 The critical current density test results of Sn superconducting materials show that Nb 3 The critical current density J of Sn superconducting material at 4.2K c (Unit: A / mm 2 ) changes with the magnetic field (unit: T). As can be seen from the figure, the Nb obtained in Example 8 3 J of Sn superconducting material in the whole tested magnetic field range c The average particle size of the raw material Nb powder is too large, which will lead to the Nb 3 J of Sn superconducting materials c This is because the excessive particle size of the raw material Nb powder will increase the diffusion distance of Sn, which makes the reaction between Nb and Sn insufficient within the same heat treatment time, resulting in the generated Nb 3 The Sn superconducting phase content is significantly reduced. Therefore, when using the heat treatment method of the present invention, it is also necessary to reasonably control the average particle size of the raw material Nb powder.
[0113] Example 9
[0114] The difference between this embodiment and embodiment 2 is that the average particle size of the elemental Nb powder in step (1) is changed to 100 nm.
[0115] The remaining steps and conditions are the same as those in Example 2.
[0116] The Nb obtained in Example 9 was tested using the test method described above. 3 Critical current density of Sn superconducting material.
[0117] Fig. 9 The Nb obtained in Example 9 and Example 2 is shown. 3 The critical current density test results of Sn superconducting materials show that Nb 3 The critical current density J of Sn superconducting material at 4.2K c (Unit: A / mm 2 ) changes with the magnetic field (unit: T). As can be seen from the figure, the Nb obtained in Example 9 3 J of Sn superconducting material in the whole tested magnetic field range c The average particle size of the raw material Nb powder is too small, which will lead to the Nb 3 J of Sn superconducting materials c This is because the small raw material Nb powder particle size will agglomerate during the cold pressing process, thus forming some large-sized Nb blocks, which usually cannot react completely, resulting in the generated Nb 3 The Sn superconducting phase content is reduced. Therefore, when adopting the heat treatment method of the present invention, it is also necessary to reasonably control the average particle size of the raw material Nb powder.
[0118] Comparative Example 1
[0119] This embodiment provides a method for preparing Nb by rapid heating 3 The method for Sn superconducting material comprises the following steps:
[0120] (1) adding elemental Nb powder, elemental Sn powder and elemental Cu powder into a mortar in a molar ratio of 3:1:3, and adding anhydrous ethanol, wherein the volume ratio of the total volume of the elemental Nb powder, elemental Sn powder and elemental Cu powder to the anhydrous ethanol is 1:2, and wet grinding is performed in the mortar for 40 minutes to obtain a mixed powder; wherein the purity of the elemental Nb powder, elemental Sn powder and elemental Cu powder is independently 99.95wt.%; the average particle size of the elemental Nb powder is 5μm; the average particle size of the elemental Sn powder and elemental Cu powder is 50μm;
[0121] (2) providing a stainless steel tube with one end open and the other end closed, the stainless steel tube being cylindrical in shape, the height of the stainless steel tube being 40 mm, the outer diameter being 20 mm, and the inner diameter being 20% smaller than the outer diameter; and providing a metal tantalum sheet having a size of 50 mm×30 mm×30 μm; curling the metal tantalum sheet into a cylindrical shape and placing it in the inner cavity of the stainless steel tube, and making the metal tantalum sheet close to the inner cavity side wall of the stainless steel tube, and then loading 20 g of the mixed powder into the inner cavity of the stainless steel tube, and then placing the copper column in the inner cavity of the stainless steel tube. The copper column is shaped like a cylinder, has a height of 30 mm, has a diameter 3% smaller than the inner diameter of the stainless steel tube, and is made of T2 copper. A pressure of 20 t is then applied to the copper column on a tablet press to perform cold pressing so that the open end of the stainless steel tube is closed to obtain a block product, wherein the block product includes a Nb-Sn-Cu block and an external coating coated on the surface of the Nb-Sn-Cu block, wherein the external coating consists of a stainless steel tube, a metal tantalum sheet, and a copper column;
[0122] (3) placing the block product obtained in step (2) in a tubular furnace and subjecting it to heat treatment in a flowing argon atmosphere, wherein the heat treatment process is as follows: heating the temperature to 580°C at a heating rate of 30°C / h, keeping the temperature for 60h, and then naturally cooling the temperature to 25°C in the furnace; then cutting the block product after the heat treatment with an electric spark cutting machine to remove the external coating to obtain Nb 3 Sn superconducting material.
[0123] Fig.10 The Nb obtained in Comparative Example 1 is shown. 3 SEM microstructure of Sn superconducting material, combined with Fig.10 and Figure 5 It can be seen that the Nb obtained in Comparative Example 1 3 There is still a lot of Nb in the Sn superconducting material that does not participate in the reaction, resulting in white Nb 3 The content of Sn superconducting phase is obviously less than that of Nb obtained in Example 5 3 Sn superconducting material, which shows that the rapid heating and short-term holding time of the second heat treatment step can significantly promote the Nb 3 The formation of Sn superconducting phase is a key step in the heat treatment process.
[0124] The Nb obtained in Comparative Example 1 and Example 5 were tested using the test method described above. 3 Critical current density of Sn superconducting material.
[0125] Fig.11 The Nb obtained in Comparative Example 1 and Example 5 is shown. 3 The critical current density of Sn superconducting materials (J c ) test results, showing Nb 3The critical current density J of Sn superconducting material at 4.2K c (Unit: A / mm 2 ) changes with the magnetic field (unit is T). As can be seen from the figure, the Nb obtained in Comparative Example 1 3 J of Sn superconducting material in the whole tested magnetic field range c The results are significantly lower than those in Example 5, which indicates that rapid heating and short-term heat preservation can significantly increase the Nb 3 J of Sn superconducting materials c .
[0126] Comparative Example 2
[0127] The difference between this comparative example and Example 2 is that the heating rate of the second heat treatment in step (3) is changed to 0.2°C / s.
[0128] The remaining steps and conditions are the same as those in Example 2.
[0129] The Nb obtained in Comparative Example 2 was tested using the test method described above. 3 Critical current density of Sn superconducting material.
[0130] Fig.12 The Nb obtained in Comparative Example 2 and Example 2 is shown. 3 The critical current density of Sn superconducting materials (J c ) test results, showing Nb 3 The critical current density J of Sn superconducting material at 4.2K c (Unit: A / mm 2 ) changes with the magnetic field (unit is T). As can be seen from the figure, the Nb obtained in Comparative Example 2 3 J of Sn superconducting material in the whole tested magnetic field range c The results are significantly lower than those in Example 2. This is because when the heating rate of the second heat treatment is low, the heat treatment time will be increased, which makes Nb 3 The Sn grains grow significantly, which leads to a decrease in the magnetic flux pinning force, which in turn leads to a decrease in J c Therefore, the heating rate of the second heat treatment needs to be reasonably controlled.
[0131] Comparative Example 3
[0132] The difference between this comparative example and Example 2 is that the heating rate of the second heat treatment in step (3) is changed to 5°C / s.
[0133] The remaining steps and conditions are the same as those in Example 2.
[0134] The Nb obtained in Comparative Example 3 was tested using the test method described above. 3 Critical current density of Sn superconducting material.
[0135] Fig.13 The Nb obtained in Comparative Example 3 and Example 2 is shown. 3 The critical current density of Sn superconducting materials (J c ) test results, showing Nb 3 The critical current density J of Sn superconducting material at 4.2K c (Unit: A / mm 2 ) changes with the magnetic field (unit is T). As can be seen from the figure, the Nb obtained in Comparative Example 2 3 J of Sn superconducting material in the whole tested magnetic field range c The results are significantly lower than those in Example 2. This is because when the heating rate of the second heat treatment is large, the heat treatment time is too short, which leads to insufficient reaction between Nb and Sn, and the generated Nb 3 The Sn superconducting phase content is significantly reduced, resulting in J c Therefore, the heating rate of the second heat treatment needs to be reasonably controlled.
[0136] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing Nb by rapid heating 3 Sn superconducting material method, It is characterized in that The method comprises: (1) mixing single-element Nb powder, single-element Sn powder and single-element Cu powder to obtain a mixed powder; (2) pressing the mixed powder to obtain a block product; (3) The bulk product is subjected to a first heat treatment and a second heat treatment in sequence to obtain Nb 3 Sn superconducting material; Among them, the first heat treatment includes a first heating stage, a first heat preservation stage and a first cooling stage carried out in sequence; the second heat treatment includes a second heating stage, a second heat preservation stage and a second cooling stage carried out in sequence, and the heating rate of the second heating stage is 0.5℃ / s-3℃ / s.
2. The method according to claim 1, It is characterized in that The average particle size of the single substance Nb powder in step (1) is 1 μm-8 μm; Preferably, the average particle sizes of the single-element Sn powder and the single-element Cu powder in step (1) are independently 30 μm-60 μm; Preferably, the purity of the single substance Nb powder, single substance Sn powder and single substance Cu powder is independently 99wt.%-99.99wt.%; Preferably, the molar ratio of the elemental Nb powder, the elemental Sn powder and the elemental Cu powder is 3:1:(1-6).
3. The method according to claim 1 or 2, It is characterized in that The mixing method in step (1) includes wet grinding; Preferably, the solvent used in the wet grinding comprises anhydrous ethanol; Preferably, the wet grinding time is 30 min-60 min.
4. The method according to any one of claims 1 to 3, It is characterized in that The compression molding method in step (2) includes a powder filling tube method; Preferably, the powder tube filling method comprises: (a) providing a stainless steel tube with one end open and the other end closed and a metal tantalum sheet, curling the metal tantalum sheet into a cylindrical shape and placing it in the inner cavity of the stainless steel tube, and making the metal tantalum sheet close to the inner cavity side wall of the stainless steel tube; (b) The mixed powder is loaded into the inner cavity of a stainless steel tube, and then a copper column is placed above the mixed powder, and the copper column is cold pressed to close the open end of the stainless steel tube to obtain the block product, which includes a Nb-Sn-Cu block and an external coating coated on the surface of the Nb-Sn-Cu block.
5. The method according to claim 4, It is characterized in that The shape of the stainless steel tube is cylindrical; Preferably, the height of the stainless steel tube is 20 mm-50 mm; the outer diameter of the stainless steel tube is 20 mm-30 mm; the inner diameter of the stainless steel tube is 10%-20% smaller than the outer diameter; Preferably, the size of the metal tantalum sheet is (30-80) mm×(20-30) mm×(20-50) μm; Preferably, the copper column is cylindrical in shape; Preferably, the height of the copper column is 20 mm-50 mm; the diameter of the copper column is 1%-3% smaller than the inner diameter of the stainless steel tube; Preferably, the material of the copper column includes T2 copper or oxygen-free copper; Preferably, the cold pressing pressure is 10t-20t.
6. The method according to any one of claims 1 to 5, It is characterized in that The first heat treatment is performed in a tube furnace; Preferably, the atmosphere of the first heat treatment is a protective atmosphere; Preferably, the heating rate in the first heating stage is 10°C / h-30°C / h; Preferably, the insulation temperature of the first insulation stage is 580°C-620°C; Preferably, the insulation time of the first insulation stage is 30h-60h; Preferably, the first temperature reduction stage is natural cooling to 25°C-35°C along with the furnace.
7. The method according to any one of claims 1 to 6, It is characterized in that The second heat treatment is performed in an induction heating furnace; Preferably, the atmosphere of the second heat treatment is a protective atmosphere; Preferably, the insulation temperature of the second insulation stage is 950°C-1050°C; Preferably, the insulation time of the second insulation stage is 0s-300s; Preferably, the second temperature reduction stage is natural cooling to 25°C-35°C along with the furnace.
8. The method according to any one of claims 4 to 7, It is characterized in that In step (3), after the second heat treatment, the outer coating is removed to obtain Nb 3 Sn superconducting material; Preferably, the outer covering is removed by cutting.
9. The method according to any one of claims 1 to 8, It is characterized in that The method specifically comprises the following steps: (I) adding elemental Nb powder, elemental Sn powder and elemental Cu powder into a mortar in a molar ratio of 3:1:(1-6), adding anhydrous ethanol, and wet grinding in the mortar for 30 min-60 min to obtain a mixed powder; wherein the purity of the elemental Nb powder, elemental Sn powder and elemental Cu powder is independently 99wt.%-99.99wt.%; the average particle size of the elemental Nb powder is 1μm-8μm; the average particle size of the elemental Sn powder and elemental Cu powder is independently 30μm-60μm; the volume ratio of the total volume of the elemental Nb powder, elemental Sn powder and elemental Cu powder to anhydrous ethanol is 1:(1-2); (II) providing a stainless steel tube with one end open and the other end closed, the stainless steel tube being cylindrical in shape, the height of the stainless steel tube being 20 mm to 50 mm, the outer diameter being 20 mm to 30 mm, and the inner diameter being 10% to 20% smaller than the outer diameter; and providing a metal tantalum sheet with a size of (30-80) mm × (20-30) mm × (20-50) μm; curling the metal tantalum sheet into a cylindrical shape and placing it in the inner cavity of the stainless steel tube, and making the metal tantalum sheet close to the inner cavity side wall of the stainless steel tube, and then adding 5 g to 20 g of the mixed The mixed powder is loaded into the inner cavity of a stainless steel tube, and a copper column is placed above the mixed powder, and a pressure of 10t-20t is applied to the copper column for cold pressing to close the open end of the stainless steel tube to obtain a block product, wherein the block product includes a Nb-Sn-Cu block and an external coating coated on the surface of the Nb-Sn-Cu block; wherein the shape of the copper column is cylindrical, the height of the copper column is 20mm-50mm, the diameter of the copper column is 1%-3% smaller than the inner diameter of the stainless steel tube, and the material of the copper column is T2 copper or oxygen-free copper; (III) placing the block product obtained in step (II) in a tubular furnace and performing a first heat treatment in a flowing argon atmosphere, wherein the specific process of the first heat treatment is: heating to 580°C-620°C at a heating rate of 10°C / h-30°C / h, keeping the temperature for 30h-60h, and then naturally cooling to 25°C-35°C with the furnace; then placing the block product after the first heat treatment in an induction heating furnace and performing a second heat treatment in an argon atmosphere, wherein the specific process of the second heat treatment is: heating to 950°C-1050°C at a heating rate of 0.5°C / s-3°C / s, keeping the temperature for 0s-300s, and then naturally cooling to 25°C-35°C with the furnace; then cutting the block product after the second heat treatment using an electric spark cutting device to remove the external coating to obtain Nb 3 Sn superconducting material.
10. A Nb 3 Sn superconducting material, It is characterized in that The Nb 3 The Sn superconducting material is prepared by the method according to any one of claims 1-9.
Citation Information
Cited By
Method for preparing internal tin method Nb3Sn superconducting wire through dieless stretching
CN121528639A