Preparation method of soft magnetic powder core material

By heat treatment and passivation of soft magnetic powder and mixed with the coating liquid to form, the problems of high loss and low magnetic permeability of soft magnetic powder core are solved, the preparation of high-performance magnetic powder core is realized, and the use of magnetic powder core is improved performance.

CN119028726APending Publication Date: 2024-11-26HENGDIAN GRP DMEGC MAGNETICS CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310600543.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing soft magnetic powder cores have problems such as high loss, serious heat generation and low effective magnetic permeability.

Method used

A specific preparation method is adopted, including first heat treatment, cooling treatment and passivation treatment of the soft magnetic powder, followed by mixing, drying and crushing screening with the coating liquid, finally molding and second heat treatment, through a specific heat treatment process and The coating is combined to improve the performance of the magnetic powder core.

Benefits of technology

It reduces the loss of the magnetic powder core, improves the effective magnetic permeability, improves the performance of the magnetic powder core, and achieves better magnetic performance and a wider application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004248797280000131
    Figure BDA0004248797280000131
Patent Text Reader

Abstract

The invention relates to a preparation method of a soft magnetic powder core material, which comprises the following steps: sequentially carrying out first heat treatment, cooling treatment and passivating treatment on soft magnetic powder to obtain treated soft magnetic powder; mixing the treated soft magnetic powder and the coating glue solution, and then drying, crushing and screening to obtain insulating treated magnetic powder; and the magnetic powder subjected to insulation treatment is subjected to forming treatment and then subjected to second heat treatment to obtain the soft magnetic powder core material. According to the preparation method provided by the invention, the preparation process is designed, and the specific heat treatment process is matched with coating, so that the preparation of the high-performance magnetic powder core material is realized, the loss of the magnetic powder core is reduced, meanwhile, the effective magnetic conductivity is improved, and the use performance of the magnetic powder core is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of powder core preparation, and in particular to a method for preparing a soft magnetic powder core material. Background Art

[0002] At present, with the development of science and technology, various types of soft magnetic powder cores are widely used in new energy, electrical, communication, automotive industry and other fields. Various types of soft magnetic powder cores tend to develop in the direction of miniaturization, intelligence, high integration and low loss.

[0003] At present, there are mainly various types of soft magnetic powder cores, such as iron powder core and metal powder core. Among them, iron powder core has higher saturation magnetic induction intensity, but lower resistivity. It is usually used in low frequency bands and has large eddy current losses at high frequencies. Although the loss of metal powder core is greatly reduced compared with that of iron powder core, its DC superposition characteristics and high-frequency losses still limit its large-scale application. The main metal powder core used is iron silicon powder core. Although iron silicon powder core has lower cost, it has high DC superposition performance.

[0004] CN104795195A discloses a sendust magnetic powder core, wherein the magnetic powder used in the sendust magnetic powder core includes the following components by weight percentage: Si, 9%-10%; Al, 5%-6%; Fe, the balance; according to the above magnetic powder ratio, the sendust magnetic powder core is prepared according to the following steps: S1: powder pre-annealing; S2: screening; S3: passivation treatment; S4: insulation coating treatment; S5: compression molding; S6: heat treatment; the sendust magnetic powder core is obtained. In the present invention, by optimizing the preparation process of the sendust magnetic powder core, each preparation step is controlled, and by the coordination of each step, the magnetic powder core can obtain excellent comprehensive performance.

[0005] For example, CN113035541A discloses a method for manufacturing an iron silicon magnetic powder core; the method for coating iron silicon powder with modified silica sol of the present invention comprises steps 1 to 9, and the method for manufacturing an iron silicon magnetic powder core of the present invention comprises steps A to E. The present invention uses a modified silica sol coating liquid to improve the performance of iron silicon powder, so that the iron silicon powder has excellent magnetic properties. The iron silicon magnetic powder core manufactured with the iron silicon powder improves the density and effective magnetic permeability of the iron silicon magnetic powder core, so that the iron silicon magnetic powder core has more excellent magnetic properties, greatly reduces the loss, greatly improves the efficiency, and reduces the energy waste. The iron silicon magnetic powder core of the present invention can be used in a higher temperature environment and has a wide range of applications.

[0006] However, the magnetic powder core disclosed in the prior art still has the problems of high loss, severe heat generation and low effective magnetic permeability. Summary of the invention

[0007] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for preparing a soft magnetic powder core material to solve the problems of high loss, severe heat generation and low effective magnetic permeability of the existing magnetic powder core.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for preparing a soft magnetic powder core material, the method comprising: subjecting the soft magnetic powder to a first heat treatment, a temperature reduction treatment and a passivation treatment in sequence to obtain a treated soft magnetic powder;

[0010] The treated soft magnetic powder and the coating glue are mixed, and then dried, crushed and sieved to obtain the insulating treated magnetic powder;

[0011] The insulation treated magnetic powder is subjected to molding treatment and then to a second heat treatment to obtain a soft magnetic powder core material.

[0012] The preparation method provided by the present invention realizes the preparation of high-performance magnetic powder core materials by designing the preparation process and adopting a specific heat treatment process and coating in combination, reduces the loss of the magnetic powder core, and at the same time achieves an improvement in the effective magnetic permeability, thereby improving the performance of the magnetic powder core.

[0013] As a preferred technical solution of the present invention, the soft magnetic powder includes iron silicon magnetic powder.

[0014] Preferably, the soft magnetic powder is prepared by aerosolization.

[0015] Preferably, the average particle size of the soft magnetic powder is 10-40 μm.

[0016] In the present invention, the average particle size of the soft magnetic powder can be an aggregate of particles within a small range within a limited range, such as all solid particles within the range of 10-25μm, or all solid particles within the range of 20-30μm, or all solid particles within the range of 30-40μm, or all solid particles within the range of 15-40μm, etc., or it can be an aggregate of particles of a single particle size within a limited range, such as an aggregate of particles with a particle size of 15μm, an aggregate of particles with a particle size of 10μm, an aggregate of particles with a particle size of 25μm, an aggregate of particles with a particle size of 30μm, an aggregate of particles with a particle size of 40μm, etc., but is not limited to the examples listed, and other unlisted values ​​within the range are equally applicable.

[0017] As a preferred technical solution of the present invention, the first heat treatment is performed under vacuum or protective atmosphere.

[0018] In the present invention, when the first heat treatment is performed under vacuum, the absolute vacuum degree can be controlled to be 0.01-0.08Pa.

[0019] In the present invention, when the first heat treatment is performed under a protective atmosphere, the protective atmosphere can be hydrogen, nitrogen, argon, helium, neon or other gases that do not react with the soft magnetic material.

[0020] Preferably, the holding temperature of the first heat treatment is 650-800°C, for example, it can be 650°C, 660°C, 670°C, 680°C, 690°C, 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C or 800°C, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0021] Preferably, the holding time of the first heat treatment is 2-3h, for example, it can be 2h, 2.1h, 2.2h, 2.3h, 2.4h, 2.5h, 2.6h, 2.7h, 2.8h, 2.9h or 3h, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0022] As a preferred technical solution of the present invention, the cooling treatment is to cool the furnace to 25-30°C at a cooling rate of ≤30°C / h.

[0023] In the present invention, the cooling rate of the cooling treatment is ≤30°C / h, for example, it can be 29°C / h, 28°C / h, 26°C / h, 24°C / h, 22°C / h, 20°C / h, 18°C / h, 16°C / h, 14°C / h, 12°C / h, 10°C / h, 8°C / h, 6°C / h, 4°C / h or 2°C / h, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0024] As a preferred technical solution of the present invention, the passivation treatment is to treat the soft magnetic powder with a phosphorus-containing reagent.

[0025] Preferably, the phosphorus-containing reagent comprises phosphoric acid and / or aluminum dihydrogen phosphate.

[0026] In the present invention, the mass percentage concentration of the phosphoric acid used is 98%, that is, commercially available analytical pure phosphoric acid.

[0027] In the present invention, the passivation treatment also includes a certain solvent such as one or more mixed solutions including but not limited to deionized water, acetone, and anhydrous ethanol. The amount of solvent required is to be able to completely immerse the magnetic powder in the solvent.

[0028] Preferably, the amount of the phosphorus-containing reagent is 0.1-1% of the mass of the soft magnetic powder;

[0029] Preferably, the passivation treatment is followed by drying.

[0030] In the present invention, the drying method after the passivation treatment includes natural drying, heating drying, vacuum drying, etc.

[0031] As a preferred technical solution of the present invention, the coating glue comprises, by mass percentage: 50-80% aqueous inorganic nano solution, 0.1-3% modifier, and the remainder is a modification auxiliary agent;

[0032] In the present invention, the mass percentage of the aqueous inorganic nano solution in the coating glue is 50-80%, for example, it can be 50%, 52%, 54%, 56%, 58%, 60%, 62%, 64%, 66%, 68%, 70%, 72%, 74%, 76%, 78% or 80%, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0033] In the present invention, the mass percentage of the modifier in the coating glue is 0.1-3%, for example, it can be 0.1%, 0.2%, 0.4%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.6%, 2.8% or 3%, etc., but is not limited to the listed values, and other values ​​not listed in the range are also applicable.

[0034] Preferably, the aqueous inorganic nano-solution comprises one or a combination of at least two of silica sol, aluminum sol, titanium sol, magnesium sol or calcium sol. The colloidal particles in the sol may be at least one of SiO2, Al2O3, TiO2, MgO, CaO, etc., preferably at least SiO2, which has a better insulating effect than the other several.

[0035] Preferably, the particle size of the colloidal particles in the aqueous inorganic nano solution is ≤100nm; setting the particle size of the insulating colloidal particles to ≤100nm can make the insulating particles adsorbed on the surface of the iron silicon magnetic powder, increase the insulation effect of the magnetic powder, and reduce the loss. Specifically, the particle size selection of the colloidal particles can be a specific aggregate of all particles in a smaller range within a limited range, or an aggregate of particles of a single particle size, such as all particle aggregates within the range of 80-90nm, all particle aggregates within the range of 40-60nm, all particle aggregates within the range of 20-40nm, all particle aggregates within the range of 10-50nm, or particle aggregates with a particle size of 20nm, particle aggregates with a particle size of 30nm, particle aggregates with a particle size of 40nm, particle aggregates with a particle size of 50nm, particle aggregates with a particle size of 60nm, particle aggregates with a particle size of 70nm, etc., but not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0036] Preferably, the modifier comprises a silane coupling agent and / or a surfactant.

[0037] In the present invention, the silane coupling agent may be a siloxane compound containing an epoxy group, and the surfactant may be a low molecular weight polyvinyl alcohol and / or a polyether-siloxane copolymer.

[0038] Preferably, the modification aid comprises polyurethane.

[0039] In the present invention, the coating glue solution can be prepared as follows: adding the modifying aid and the modifier into the aqueous inorganic nano-solution, and then stirring and mixing at a certain temperature, wherein the time is 0.5-5h and the temperature is 15-40°C.

[0040] Preferably, the amount of the coating glue is 1-2% of the mass of the soft magnetic powder, for example, it can be 1%, 1.05%, 1.1%, 1.15%, 1.2%, 1.25%, 1.3%, 1.35%, 1.4%, 1.45%, 1.5%, 1.55%, 1.6%, 1.65%, 1.7%, 1.75%, 1.8%, 1.85%, 1.9%, 1.95% or 2%, etc., but is not limited to the listed values, and other values ​​not listed in this range are also applicable.

[0041] In the present invention, a certain solvent is added during the mixing of the soft magnetic powder and the coating glue, such as acetone and / or anhydrous ethanol, which has good solubility with the glue and a low boiling point, and is preferably required to be able to completely soak the magnetic powder into the solvent. The mixing time can be 2-5 minutes, and the drying after mixing can be natural drying, heating drying, vacuum drying, etc.

[0042] As a preferred technical solution of the present invention, the mesh size of the screen used in the crushing and screening is 80-140 mesh, for example, it can be 80 mesh, 90 mesh, 100 mesh, 110 mesh, 120 mesh, 130 mesh or 140 mesh, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0043] As a preferred technical solution of the present invention, the molding process is to mix the insulating treated magnetic powder and the release agent and then perform compression molding;

[0044] Preferably, the release agent comprises zinc stearate;

[0045] Preferably, the amount of the release agent is 0.2-0.6% of the mass of the insulated magnetic powder, for example, it can be 0.2%, 0.22%, 0.24%, 0.26%, 0.28%, 0.3%, 0.32%, 0.34%, 0.36%, 0.38%, 0.4%, 0.42%, 0.44%, 0.46%, 0.48%, 0.5%, 0.52%, 0.54%, 0.56%, 0.58% or 0.6%, etc., but is not limited to the listed values, and other values ​​not listed in this range are also applicable.

[0046] Preferably, the molding pressure in the molding process is 1500-2000MPa, for example, it can be 1500MPa, 1550MPa, 1600MPa, 1650MPa, 1700MPa, 1750MPa, 1800MPa, 1850MPa, 1900MPa, 1950MPa or 2000MPa, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0047] As a preferred technical solution of the present invention, the insulation temperature of the second heat treatment is 680-720°C, for example, it can be 680°C, 682°C, 684°C, 686°C, 688°C, 690°C, 692°C, 694°C, 696°C, 698°C, 700°C, 702°C, 704°C, 706°C, 708°C, 710°C, 712°C, 714°C, 716°C, 718°C or 720°C, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0048] Preferably, the holding time of the second heat treatment is 1-2h, for example, it can be 1h, 1.05h, 1.1h, 1.15h, 1.2h, 1.25h, 1.3h, 1.35h, 1.4h, 1.45h, 1.5h, 1.55h, 1.6h, 1.65h, 1.7h, 1.75h, 1.8h, 1.85h, 1.9h, 1.95h or 2h, but is not limited to the listed values, and other values ​​not listed in the range are also applicable.

[0049] Preferably, the second heat treatment is performed under an inert atmosphere; the inert atmosphere includes nitrogen and / or a rare gas, and the rare gas may be helium, neon, argon, etc.

[0050] Preferably, furnace cooling is performed after the second heat treatment is completed.

[0051] In the present invention, after the second heat treatment is completed, the furnace is cooled to room temperature, such as 25-30°C.

[0052] As a preferred technical solution of the present invention, the preparation method comprises: subjecting the soft magnetic powder to a first heat treatment, a temperature reduction treatment and a passivation treatment in sequence to obtain a treated soft magnetic powder;

[0053] The treated soft magnetic powder and the coating glue are mixed, and then dried, crushed and sieved to obtain the insulating treated magnetic powder;

[0054] The insulating treated magnetic powder is subjected to a molding process and then subjected to a second heat treatment to obtain a soft magnetic powder core material;

[0055] Wherein, the soft magnetic powder includes ferrosilicon magnetic powder; the soft magnetic powder is prepared by atomization; the average particle size of the soft magnetic powder is 10-40μm; the first heat treatment is carried out in vacuum or protective atmosphere; the insulation temperature of the first heat treatment is 650-800℃; the insulation time of the first heat treatment is 2-3h; the cooling treatment is to cool down to 25-30℃ with the furnace at a cooling rate of ≤30℃ / h; the passivation treatment is to treat the soft magnetic powder with a phosphorus-containing reagent; the phosphorus-containing reagent includes phosphoric acid and / or aluminum dihydrogen phosphate; the amount of the phosphorus-containing reagent is 0.1-1% of the mass of the soft magnetic powder; the passivation treatment is followed by drying; the coating glue solution includes, by mass percentage: 50-80% aqueous inorganic nano solution, 0.1-3% modifier, and the remainder is a modification aid; the aqueous inorganic nano solution includes silica sol, aluminum sol, titanium sol, A combination of one or at least two of magnesium sol or calcium sol; the particle size of the colloidal particles in the aqueous inorganic nano solution is ≤100nm; the modifier includes a silane coupling agent and / or a surfactant; the modification aid includes polyurethane; the amount of the coating glue is 1-2% of the mass of the soft magnetic powder; the mesh size of the screen used in the crushing and screening is 80-140 meshes; the molding process is to mix the insulation-treated magnetic powder and the release agent and then press-form; the release agent includes zinc stearate; the amount of the release agent is 0.2-0.6% of the mass of the insulation-treated magnetic powder; the molding pressure in the molding process is 1500-2000MPa; the insulation temperature of the second heat treatment is 680-720℃; the insulation time of the second heat treatment is 1-2h; the second heat treatment is carried out in an inert atmosphere; and the second heat treatment is cooled with the furnace after completion.

[0056] Compared with the prior art solutions, the present invention has the following beneficial effects:

[0057] The preparation method provided by the present invention adopts a specific processing process to make the insulating silicon particles more easily adsorbed to the surface of the magnetic powder to achieve a better insulation effect, thereby reducing the loss of the magnetic powder core. It can also improve the density and effective magnetic permeability of the iron-silicon magnetic powder core, so that the iron-silicon magnetic powder core has better magnetic properties, greatly improves efficiency, and reduces energy waste. The initial magnetic permeability of the obtained soft magnetic powder core is ≥60, and the loss Pcv is ≤455mW / cm3 . DETAILED DESCRIPTION

[0058] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0059] Example 1

[0060] This embodiment provides a method for preparing a soft magnetic powder core material, which specifically includes the following steps:

[0061] (1) First heat treatment and cooling treatment

[0062] The iron silicon magnetic powder (average particle size of 13 μm) obtained by gas atomization was selected and placed in a heat treatment furnace. The furnace temperature was raised to 740°C and kept warm for 2 hours. Then the temperature was slowly lowered to room temperature (30°C) and taken out of the furnace. The cooling rate was 30°C / h. The atmosphere in the furnace could be vacuum, and the absolute vacuum degree was 0.03Pa.

[0063] (2) Passivation treatment

[0064] The magnetic powder after the heat treatment in step (1) is fully mixed with phosphoric acid (mass concentration is 98%) and acetone, and then dried to obtain passivated magnetic powder.

[0065] The amount of phosphoric acid used is 0.2% of the alloy magnetic powder, which can completely soak the magnetic powder into the solvent, and the powder is heated and dried while being stirred, and the drying temperature is 80°C.

[0066] (3) Coating and bonding

[0067] The coating glue solution includes the following components: 65% silica sol; 1% silane coupling agent; 34% organic silicone resin;

[0068] The preparation method is as follows: polyurethane resin and silane coupling agent are added into silica sol, and then stirred and mixed at a certain temperature, wherein the time is 2 hours and the temperature is 25°C.

[0069] In the coating colloid solution, the particle size of the colloid particles is ≤20nm.

[0070] The magnetic powder obtained in step (2) is fully mixed with the coating glue and solvent, and then dried. The completely dried magnetic powder is crushed and sieved to obtain coated magnetic powder for standby use.

[0071] The coating glue is used in an amount of 1.5% of the mass of the iron silicon magnetic powder; the solvent is acetone, which can completely soak the magnetic powder into the solvent; the drying is carried out by natural drying. The mesh number of the sieve is 100 meshes.

[0072] (4) Pressing treatment

[0073] The magnetic powder obtained in step (3) is fully mixed with a release agent and placed in a press for molding.

[0074] The demoulding agent is zinc stearate, and the dosage is 0.4% of the mass of the magnetic powder. The molding pressure is 1900 MPa.

[0075] (5) Second heat treatment

[0076] The magnet obtained in step (4) is placed in a furnace for heat treatment, and the heat treatment is carried out under nitrogen protection.

[0077] The heat treatment temperature process parameters are as follows: raise the furnace temperature to 700°C, keep it warm for 1 hour, cool it to room temperature (25°C) with the furnace, and take it out for testing.

[0078] In order to facilitate testing during the pressing process, the sample to be tested is directly pressed, specifically, a magnetic ring with an outer diameter of 12.7mm, an inner diameter of 7.6mm, and a height of 3mm is pressed. The density ρ of the magnetic core is tested by the drainage method. The magnetic core is subsequently wound and the inductance L is tested by an LCR meter. The effective magnetic permeability μ of the ring core is calculated. The test frequency is 100kHz. The Japanese Iwasaki SY-8218 soft magnetic BH analyzer is used to test the AC loss of the magnetic core. The test conditions are: 50kHz, 100mT, and temperature is 25℃.

[0079] Example 2

[0080] The only difference from Example 1 is that the aqueous inorganic nano-solution is selected as aluminum sol.

[0081] Example 3

[0082] The only difference from Example 1 is that the aqueous inorganic nano-solution is selected as calcium sol.

[0083] Example 4

[0084] The only difference from Example 1 is that the aqueous inorganic nano-solution is selected as titanium sol.

[0085] Table 1 below shows the test results of Examples 1 to 4. From the results of the Examples, it can be seen that among the insulating colloidal particles SiO2, Al2O3, TiO2, and CaO, SiO2 has the best effect.

[0086] Table 1

[0087] μ <![CDATA[Pcv(mW / cm 3 )]]> <![CDATA[ρ(g / cm 3 )]]> Example 1 80 380 6.70 Example 2 75 420 6.55 Example 3 70 430 6.50 Example 4 72 410 6.60

[0088] Example 5

[0089] This embodiment provides a method for preparing a soft magnetic powder core material, which specifically includes the following steps:

[0090] (1) First heat treatment and cooling treatment

[0091] The iron silicon magnetic powder (average particle size of 40 μm) obtained by gas atomization is selected and placed in a heat treatment furnace. The furnace temperature is raised to 700°C and kept warm for 3 hours. Then the temperature is slowly lowered to room temperature (25°C) and taken out of the furnace. The cooling rate is 30°C / h. The atmosphere in the furnace can be vacuum, and the absolute vacuum degree is 0.08Pa.

[0092] (2) Passivation treatment

[0093] The magnetic powder after the heat treatment in step (1) is fully mixed with phosphoric acid (mass concentration is 98%) and acetone, and then dried to obtain passivated magnetic powder.

[0094] The amount of phosphoric acid used is 0.2% of the alloy magnetic powder, which can completely soak the magnetic powder into the solvent, and the powder is heated and dried while being stirred, and the drying temperature is 80°C.

[0095] (3) Coating and bonding

[0096] The coating glue solution includes the following components: 65% silica sol; 1% silane coupling agent; 34% organic silicone resin;

[0097] The preparation method is as follows: polyurethane resin and silane coupling agent are added into silica sol, and then stirred and mixed at a certain temperature, wherein the time is 2 hours and the temperature is 25°C.

[0098] In the coating colloid solution, the particle size of the colloid particles is ≤20nm.

[0099] The magnetic powder obtained in step (2) is fully mixed with the coating glue and solvent, and then dried. The completely dried magnetic powder is crushed and sieved to obtain coated magnetic powder for standby use.

[0100] The coating glue is used in an amount of 1.5% of the mass of the iron silicon magnetic powder; the solvent is acetone, which can completely soak the magnetic powder into the solvent; the drying is carried out by natural drying. The mesh number of the sieve is 140 meshes.

[0101] (4) Pressing treatment

[0102] The magnetic powder obtained in step (3) is fully mixed with a release agent and placed in a press for molding.

[0103] The demoulding agent is zinc stearate, and the dosage is 0.3% of the mass of the magnetic powder. The molding pressure is 1700 MPa.

[0104] (5) Second heat treatment

[0105] The magnet obtained in step (4) is placed in a furnace for heat treatment, and the heat treatment is carried out under nitrogen protection.

[0106] The heat treatment temperature process parameters are as follows: raise the furnace temperature to 700°C, keep it warm for 1 hour, cool it to room temperature (30°C) with the furnace, and take it out for testing.

[0107] In order to facilitate testing during the pressing process, the sample to be tested is directly pressed, specifically, a magnetic ring with an outer diameter of 12.7mm, an inner diameter of 7.6mm, and a height of 3mm is pressed. The density ρ of the magnetic core is tested by the drainage method. The magnetic core is subsequently wound and the inductance L is tested by an LCR meter. The effective magnetic permeability μ of the ring core is calculated. The test frequency is 100kHz. The Japanese Iwasaki SY-8218 soft magnetic BH analyzer is used to test the AC loss of the magnetic core. The test conditions are: 50kHz, 100mT, and temperature is 25℃.

[0108] Example 6

[0109] The only difference from Example 5 is that the first heat treatment is not performed.

[0110] Example 7

[0111] The only difference from Example 5 is that the temperature of the first heat treatment is 780°C.

[0112] Example 8

[0113] The only difference from Example 5 is that the temperature of the first heat treatment is 820°C.

[0114] Example 9

[0115] The only difference from Example 5 is that the cooling rate is 40° C. / h.

[0116] Table 2 below shows the test results of Examples 5-9. From the results of Example 6, it can be seen that

[0117] The comprehensive performance of the magnetic cores that are not pretreated before passivation is reduced, especially in terms of loss. This is mainly because reasonable pretreatment can improve the microstructure inside the magnetic powder and reduce the surface hardness of the magnetic powder, which is more conducive to the increase of density in the subsequent pressing process, thereby improving the magnetic properties of the magnetic core. From the results of comparative examples 7-9, the pretreatment temperature and cooling rate should be controlled within a certain range. This is mainly because too low a temperature cannot achieve the purpose of improving the microstructure, while too high a temperature will lead to the generation of new phases, and too fast a cooling rate will cause stress inside the magnetic powder again, which is not conducive to the improvement of the magnetic powder's plastic deformation ability. In short, pretreatment is very necessary, and the insulation temperature and cooling rate need to be controlled within a certain range.

[0118] Table 2

[0119]

[0120]

[0121] Example 10

[0122] This embodiment provides a method for preparing a soft magnetic powder core material, which specifically includes the following steps:

[0123] (1) First heat treatment and cooling treatment

[0124] Iron silicon magnetic powder (average particle size of 15 μm) obtained by gas atomization is selected and placed in a heat treatment furnace. The furnace temperature is raised to 720°C and kept warm for 2 hours. Then the temperature is slowly lowered to room temperature (25°C) and taken out of the furnace. The cooling rate is 30°C / h. The atmosphere in the furnace can be vacuum, and the absolute vacuum degree is 0.02Pa.

[0125] (2) Passivation treatment

[0126] The magnetic powder after the heat treatment in step (1) is fully mixed with phosphoric acid (mass concentration is 98%) and acetone, and then dried to obtain passivated magnetic powder;

[0127] The amount of phosphoric acid used is 0.2% of the alloy magnetic powder, which can completely soak the magnetic powder into the solvent, and the powder is heated and dried while being stirred, and the drying temperature is 80°C.

[0128] (3) Coating and bonding

[0129] The coating glue solution includes the following components: 65% silica sol; 1% silane coupling agent; 34% organic silicone resin;

[0130] The preparation method is as follows: polyurethane resin and silane coupling agent are added into silica sol, and then stirred and mixed at a certain temperature, wherein the time is 2 hours and the temperature is 25°C.

[0131] In the coating colloid solution, the particle size of the colloid particles is ≤20nm.

[0132] The magnetic powder obtained in step (2) is fully mixed with the coating glue and solvent, and then dried. The completely dried magnetic powder is crushed and sieved to obtain coated magnetic powder for standby use.

[0133] The coating glue is used in an amount of 1.5% of the mass of the iron silicon magnetic powder; the solvent is acetone, which can completely soak the magnetic powder into the solvent; the drying is carried out by natural drying. The mesh number of the sieve is 120 meshes.

[0134] (4) Pressing treatment

[0135] The magnetic powder obtained in step (3) is fully mixed with a release agent and placed in a press for molding.

[0136] The demoulding agent is zinc stearate, and the dosage is 0.3% of the mass of the magnetic powder. The molding pressure is 1800 MPa.

[0137] (5) Second heat treatment

[0138] The magnet obtained in step (4) is placed in a furnace for heat treatment, and the heat treatment is carried out under nitrogen protection.

[0139] The heat treatment temperature process parameters are as follows: raise the furnace temperature to 700°C, keep it warm for 1 hour, cool it to room temperature (25°C) with the furnace, and take it out for testing.

[0140] In order to facilitate testing during the pressing process, the sample to be tested is directly pressed, specifically, a magnetic ring with an outer diameter of 12.7mm, an inner diameter of 7.6mm, and a height of 3mm is pressed. The density ρ of the magnetic core is tested by the drainage method. The magnetic core is subsequently wound and the inductance L is tested by an LCR meter. The effective magnetic permeability μ of the ring core is calculated. The test frequency is 100kHz. The Japanese Iwasaki SY-8218 soft magnetic BH analyzer is used to test the AC loss of the magnetic core. The test conditions are: 50kHz, 100mT, and temperature is 25℃.

[0141] Embodiment 11

[0142] The only difference from Example 10 is that the particle size of the silica sol is 50 nm.

[0143] Example 12

[0144] The only difference from Example 10 is that the particle size of the selected silica sol is 1 μm.

[0145] Embodiment 13

[0146] The only difference from Example 10 is that the particle size of the iron silicon magnetic powder is 100-200 μm, which refers to the aggregate of all particles within the particle size range.

[0147] Embodiment 14

[0148] The only difference from Example 10 is that the particle size of the iron silicon magnetic powder is 100-200μm, and the particle size is 10-20μm, which refers to the aggregate of all particles within the particle size range, 100-200μm accounts for 50%, and 10-20μm accounts for 50%, calculated in mass percentage.

[0149] Table 3 below shows the test results of Examples 10-14. From the results of the examples, it can be seen that as the size of the silica sol particles increases, the loss increases. This is because the adsorption effect of the particles becomes worse as the size increases, which leads to worse insulation effect and greater loss. Moreover, the larger the particles, the worse the compression effect, resulting in a smaller density.

[0150] Table 3

[0151] μ <![CDATA[Pcv(mW / cm 3 )]]> <![CDATA[ρ(g / cm 3 )]]> Example 10 82 390 6.72 Embodiment 11 73 425 6.56 Example 12 60 455 6.45 Embodiment 13 100 550 6.9 Embodiment 14 92 480 6.81

[0152] The preparation method provided by the present invention realizes the preparation of high-performance magnetic powder core materials by designing the preparation process and adopting a specific heat treatment process and coating in combination, reduces the loss of the magnetic powder core, and at the same time achieves an improvement in the effective magnetic permeability, thereby improving the performance of the magnetic powder core.

[0153] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0154] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0155] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0156] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing a soft magnetic powder core material, characterized in that: The preparation method comprises: subjecting the soft magnetic powder to a first heat treatment, a temperature reduction treatment and a passivation treatment in sequence to obtain a treated soft magnetic powder; The treated soft magnetic powder and the coating glue are mixed, and then dried, crushed and sieved to obtain the insulating treated magnetic powder; The insulation treated magnetic powder is subjected to molding treatment and then to a second heat treatment to obtain a soft magnetic powder core material.

2. The preparation method according to claim 1, characterized in that: The soft magnetic powder includes iron silicon magnetic powder; Preferably, the soft magnetic powder is prepared by aerosolization; Preferably, the average particle size of the soft magnetic powder is 10-40 μm.

3. The preparation method according to claim 1 or 2, characterized in that: The first heat treatment is performed under vacuum or protective atmosphere; Preferably, the holding temperature of the first heat treatment is 650-800°C; Preferably, the holding time of the first heat treatment is 2-3 hours.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The temperature reduction treatment is to reduce the temperature to 25-30°C with the furnace at a temperature reduction rate of ≤30°C / h.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The passivation treatment is to treat the soft magnetic powder with a phosphorus-containing reagent; Preferably, the phosphorus-containing reagent comprises phosphoric acid and / or aluminum dihydrogen phosphate; Preferably, the amount of the phosphorus-containing reagent is 0.1-1% of the mass of the soft magnetic powder; Preferably, the passivation treatment is followed by drying.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The coating glue solution comprises, by mass percentage, 50-80% aqueous inorganic nano solution, 0.1-3% modifier, and the remainder is a modification auxiliary agent; Preferably, the aqueous inorganic nano-solution comprises one or a combination of at least two of silica sol, aluminum sol, titanium sol, magnesium sol or calcium sol; Preferably, the particle size of the colloidal particles in the aqueous inorganic nano-solution is ≤100 nm; Preferably, the modifier comprises a silane coupling agent and / or a surfactant; Preferably, the modification aid comprises polyurethane; Preferably, the amount of the coating glue is 1-2% of the mass of the soft magnetic powder.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The mesh number of the screen used in the crushing and screening is 80-140 meshes.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The molding process is to mix the insulating treated magnetic powder and the release agent and then perform compression molding; Preferably, the release agent comprises zinc stearate; Preferably, the amount of the release agent is 0.2-0.6% of the mass of the insulated magnetic powder; Preferably, the molding pressure in the molding process is 1500-2000 MPa.

9. The preparation method according to any one of claims 1 to 8, characterized in that: The holding temperature of the second heat treatment is 680-720°C; Preferably, the holding time of the second heat treatment is 1-2h; Preferably, the second heat treatment is performed under an inert atmosphere; Preferably, furnace cooling is performed after the second heat treatment is completed.

10. The preparation method according to any one of claims 1 to 9, characterized in that: The preparation method comprises: subjecting the soft magnetic powder to a first heat treatment, a temperature reduction treatment and a passivation treatment in sequence to obtain a treated soft magnetic powder; The treated soft magnetic powder and the coating glue are mixed, and then dried, crushed and sieved to obtain the insulating treated magnetic powder; The insulating treated magnetic powder is subjected to a molding process and then subjected to a second heat treatment to obtain a soft magnetic powder core material; Wherein, the soft magnetic powder includes ferrosilicon magnetic powder; the soft magnetic powder is prepared by atomization; the average particle size of the soft magnetic powder is 10-40μm; the first heat treatment is carried out in vacuum or protective atmosphere; the insulation temperature of the first heat treatment is 650-800℃; the insulation time of the first heat treatment is 2-3h; the cooling treatment is to cool down to 25-30℃ with the furnace at a cooling rate of ≤30℃ / h; the passivation treatment is to treat the soft magnetic powder with a phosphorus-containing reagent; the phosphorus-containing reagent includes phosphoric acid and / or aluminum dihydrogen phosphate; the amount of the phosphorus-containing reagent is 0.1-1% of the mass of the soft magnetic powder; the passivation treatment is followed by drying; the coating glue solution includes, by mass percentage: 50-80% aqueous inorganic nano solution, 0.1-3% modifier, and the remainder is a modification aid; the aqueous inorganic nano solution includes silica sol, aluminum sol, titanium sol, A combination of one or at least two of magnesium sol or calcium sol; the particle size of the colloidal particles in the aqueous inorganic nano solution is ≤100nm; the modifier includes a silane coupling agent and / or a surfactant; the modification aid includes polyurethane; the amount of the coating glue is 1-2% of the mass of the soft magnetic powder; the mesh size of the screen used in the crushing and screening is 80-140 meshes; the molding process is to mix the insulation-treated magnetic powder and the release agent and then press-form; the release agent includes zinc stearate; the amount of the release agent is 0.2-0.6% of the mass of the insulation-treated magnetic powder; the molding pressure in the molding process is 1500-2000MPa; the insulation temperature of the second heat treatment is 680-720℃; the insulation time of the second heat treatment is 1-2h; the second heat treatment is carried out in an inert atmosphere; and the second heat treatment is cooled with the furnace after completion.

Citation Information

Cited By

  • Iron-silicon magnetic material as well as preparation method and application thereof

    CN119480406A

  • Iron-silicon magnetic material, method for preparing same and use thereof

    CN119480406B