Test structure and measurement method for copper recess
By designing a test structure containing copper blocks and test ends after copper CMP, and using electrical measurement to calculate the depression depth, the problems of damage and non-repeatability of traditional AFM methods are solved, and low-cost, repeatable copper depression measurement is achieved and accurate simulation is achieved. The sag condition after copper CMP is completed.
Patent Information
- Application Number
- CN202411114185.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The prior art is difficult to effectively and at low cost to measure the post-depression of copper CMP, and the traditional AFM method is prone to damage the metal surface and cannot be repeated.
Design a test structure for copper depressions, including regular-shaped copper blocks, test copper blocks and test ends located in the interlayer dielectric layer, calculate the depression depth through electrical measurement, and calculate the test copper block thickness using the Vanderbilt formula to achieve non-existence Destructive test.
The metal surface damage problem of AFM measurement is avoided, the testing cost is reduced, the measurement repeatability is improved, and the depression after copper CMP is accurately simulated.
Smart Images

Figure CN119028855A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor devices, and in particular to a test structure and a measurement method for copper recesses. Background Art
[0002] With the development of technology nodes, the critical dimension (CD) of the back-end metal connection is getting smaller and smaller, the resistance is getting larger and larger, and the RC delay problem is serious. To solve this problem, IBM launched the Cu interconnect in 1997. The Cu interconnect adopts the dual Damascene process, so the CMP process needs to be used to remove the excess copper blocks after Cu electroplating. However, Cu is soft in texture and is prone to dishing after CMP, which is especially serious on large copper blocks. Since Cu digging will affect the in-plane flatness of the wafer, if it is not controlled, it will have a serious impact on subsequent processes. Therefore, for the Cu CMP process, the Cu digging depth is an important control parameter, especially for large copper blocks.
[0003] To address the above problems, the traditional method for measuring Cu concavity is AFM (Atomic Force Microscope), but this method easily scratches the metal surface, the wafer needs to be scrapped after the test, the test cost is high, and it is not repeatable.
[0004] Therefore, a repeatable and low-cost method is needed to measure the dishing after Cu CMP polishing. Summary of the invention
[0005] The technical problem solved by the present invention is how to measure the concavity after Cu CMP by a method with high repeatability and low cost.
[0006] To solve the above technical problem, according to a first aspect of an embodiment of the present invention, a test structure for copper recesses is provided, wherein the test structure is located in a dicing path of a wafer and comprises:
[0007] interlayer dielectric layer;
[0008] At least four copper blocks of regular shape, at least one test copper block and at least four test ends; the four test ends extend from four corners of the test copper block; the four copper blocks of regular shape are each disposed between two of the test ends to surround the test copper block;
[0009] The copper block, the test copper block and the test end are all embedded in the interlayer dielectric layer;
[0010] The ratio of the size of the copper block to the size of the test copper block is greater than 100:1;
[0011] The distance between the test end and the copper block is greater than or equal to the minimum design rule of copper process manufacturing.
[0012] Optionally, the test structure includes n test copper blocks, which are spaced apart by a preset distance and arranged in one dimension; correspondingly, the number of the test ends and the copper blocks is 2*(n+1).
[0013] Optionally, the test structure includes m*n test copper blocks, which are spaced at a preset distance and arranged in two dimensions. Correspondingly, the number of the test ends is 2*(m+n), and the number of the copper blocks is (m+1)*(n+1).
[0014] Optionally, the test copper block is located in the middle of the overall figure formed by the copper blocks.
[0015] Optionally, the copper block is a rectangular structure, and the overall shape of a plurality of the copper blocks after being arranged is also rectangular; the test copper block arranged between the copper blocks is a rectangular shape rotated 45 degrees relative to the adjacent copper blocks.
[0016] According to a second aspect of an embodiment of the present invention, there is provided a method for measuring copper recesses using the copper recess test structure as described in the first aspect of the present invention, comprising the following steps:
[0017] Step S1: measuring the thickness of the interlayer dielectric layer located adjacent to the test structure;
[0018] Step S2: Obtain the resistivity ρ of metal copper;
[0019] Step S3: using the Van der Pauw method, combined with the copper resistivity ρ obtained in step S2, for the four test terminals of the test copper block at the test position, two adjacent test terminals are selected for the first time to pass the first test current, and the test voltage is obtained through the remaining two test terminals; two opposite test terminals are selected for the second time to pass the second test current, and the test voltage is obtained through the remaining two test terminals; one of the two opposite test terminals in the second time and the two adjacent test terminals in the first time is the same, and the thickness of the test copper block is calculated using the Van der Pauw formula;
[0020] Step S4: Subtract the thickness of the test copper block obtained in step S3 from the thickness of the interlayer dielectric layer obtained in step S1 to obtain data on the depression of the position of the test copper block relative to the interlayer dielectric layer.
[0021] Optionally, in step S1, an ellipsometer is used to measure the thickness of the interlayer dielectric layer.
[0022] Optionally, in step S2, a four-probe method is used to test the resistivity ρ of metallic copper.
[0023] Optionally, the Van der Pauw formula in step S3 is: Wherein R1=V1 / I1, R2=V2 / I2; wherein I1 is the current applied for the first time, V1 is the voltage measured for the first time, I2 is the current applied for the second time, and V2 is the voltage measured for the second time; the value of λ is calculated according to the Van der Pauw formula, and then the thickness of the test copper block is calculated according to the thickness formula: d=ρ / πλ.
[0024] Compared with the prior art, the technical solution of the embodiment of the present invention has the following beneficial effects:
[0025] The copper depression test structure provided by the present invention includes at least four copper blocks of regular shape located in the interlayer dielectric layer, at least one test copper block and at least four test terminals; using at least four test terminals, the depth of the depression on the surface of the test copper block can be calculated by means of electrical measurement, thereby avoiding the problem that the traditional AFM method of measuring surface depression easily scratches the metal surface; by changing the position of the test copper block, the measurement of the depth of the copper depression at different positions is further improved, and the morphology of the copper defect is further obtained, thereby accurately simulating the depression after copper CMP; because the test performed by the test structure of the present invention is a non-destructive test, the wafer after the test does not need to be scrapped, thereby reducing the test cost. In addition, the test structure provided by the present invention can be repeatedly measured multiple times, thereby improving repeatability. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a schematic diagram of the structure of a large piece of copper after CMP;
[0027] Figure 2 A schematic diagram of a copper recess test structure provided by an embodiment of the present invention Figure 1 ;
[0028] Figure 3 A schematic diagram of a copper recess test structure provided by an embodiment of the present invention Figure 2 ;
[0029] Figure 4 A schematic diagram of a copper recess test structure provided by an embodiment of the present invention Figure 3 ;
[0030] Figure 5 A schematic diagram of a copper recess test structure provided by an embodiment of the present invention Figure 4 ;
[0031] Figure 6 It is a coordinate schematic diagram of a copper recess test structure provided by an embodiment of the present invention;
[0032] Figure 7It is a flow chart of a method for measuring a copper recessed test structure provided by an embodiment of the present invention. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. The terms "first", "second", "third", "fourth", etc. (if any) in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described here can be implemented in an order other than those illustrated or described here. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0034] As described in the background technology, the traditional method for measuring Cu concavity is AFM, but this method easily scratches the metal surface, the wafer needs to be scrapped after the test, the test cost is high, and it is not repeatable. The following will describe the existing AFM test method in detail with reference to the accompanying drawings.
[0035] Figure 1 This is a schematic diagram of the structure of a large piece of copper after CMP.
[0036] Please refer to Figure 1 , the large copper block 1 is located in the interlayer dielectric layer, and the large copper block 1 has been subjected to CMP polishing; specifically, the interlayer dielectric layer includes, for example, a first interlayer dielectric layer 100 and a second interlayer dielectric layer 101 located on the first interlayer dielectric layer 100, and the large copper block 1 is specifically located in the second interlayer dielectric layer 101. Of course, the specific composition of the interlayer dielectric layer here is only an example, and it can also be other compositions, and this application does not make specific restrictions on this. It should be noted that the interlayer dielectric layers mentioned below all correspond to Figure 1 The second interlayer dielectric layer is the interlayer dielectric layer in which the bulk copper is embedded.
[0037] Depend on Figure 1It can be seen that after CMP, the large piece of copper 1 has surface depressions. This is because copper is soft, and this situation is particularly serious on large pieces of copper metal. Since copper surface depressions affect the in-plane flatness of the wafer, the prior art usually requires the use of AFM to measure copper surface depressions. However, this method is easy to scratch the metal surface, and the wafer needs to be scrapped after the test, so the test cost is high and it is not repeatable.
[0038] In order to solve the above problems, an embodiment of the present invention provides a test structure of copper recesses, which is located in the cutting path of a wafer and includes: an interlayer dielectric layer, at least four copper blocks of regular shapes, at least one test copper block and at least four test ends; the four test ends extend from four corners of the test copper block; the four copper blocks of regular shapes are each arranged between two of the test ends to surround the test copper block; the copper blocks, the test copper blocks and the test ends are all embedded in the interlayer dielectric layer; the ratio of the size of the copper block to the size of the test copper block is greater than 100:1; the spacing between the test end and the copper block is greater than or equal to the minimum design rule for copper process manufacturing.
[0039] The copper depression test structure provided by the embodiment of the present invention is formed in the interlayer dielectric layer by at least four copper blocks of regular shapes, at least one test copper block and at least four test terminals; using at least four test terminals, the depth of the depression on the surface of the test copper block can be calculated by means of electrical measurement, thereby avoiding the problem that the traditional AFM method of measuring surface depression easily scratches the metal surface; by changing the position of the test copper block, the measurement of the depth of the copper depression at different positions is further improved, and the morphology of the copper defect is further obtained, thereby accurately simulating the depression after copper CMP; because the test performed by the test structure of the present invention is a non-destructive test, the wafer after the test does not need to be scrapped, thereby reducing the test cost. In addition, the test structure provided by the present invention can be repeatedly measured multiple times, thereby improving repeatability.
[0040] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0041] Figure 2 A schematic diagram of a copper recess test structure provided by an embodiment of the present invention.
[0042] Please refer to Figure 2 An embodiment of the present invention provides a copper recessed test structure 10, the test structure is located in a dicing path of a wafer, and the test structure includes:
[0043] An interlayer dielectric layer 101, at least four copper blocks 102 of regular shape, at least one test copper block 103 and at least four test terminals a, b, c, d; the four test terminals a, b, c, d extend from four corners of the test copper block 103; the four copper blocks 102 of regular shape are respectively arranged between two test terminals to surround the test copper block 103.
[0044] In a specific example, the copper block 102 is a rectangular structure, and the overall shape of several copper blocks 102 after being arranged is also rectangular; the test copper block 103 arranged between the copper blocks 102 is a rectangular shape rotated 45 degrees relative to the adjacent copper block 102.
[0045] In an optional implementation, the test copper block 103 is located in the middle of the overall figure formed by the copper blocks 102, so as to measure the depth of the depression near the center point.
[0046] The copper block 102, the test copper block 103 and the test terminals a, b, c, d are all embedded in the interlayer dielectric layer 101. The ratio of the size of the copper block 102 to the size of the test copper block 103 is greater than 100:1. The spacing between the test terminal and the copper block 102 is greater than or equal to the minimum design rule of copper process manufacturing. Therefore, on the one hand, the distance between the copper blocks can be controlled to be minimum, just enough to pass the design rule checking (DRC). On the other hand, since there is only a small oxide space between the copper blocks, there is not enough resistance to polishing, so it can be approximately considered that Figure 2 The structure is similar to the depression of bulk copper after CMP, making Figure 2 The test structure can accurately simulate the depression of bulk copper after CMP.
[0047] The test structure may include n test copper blocks 103 , wherein the n test copper blocks 103 are spaced apart by a preset distance and are arranged in a one-dimensional direction; correspondingly, the number of the test ends and the copper blocks 102 is 2*(n+1).
[0048] Figure 3 and Figure 4 They are schematic diagrams of a copper recess test structure 10 provided by an embodiment of the present invention. Figure 3 or Figure 4 In a specific example, when n=2, the number of the test terminals and the number of the copper blocks 102 are both 6. If it is necessary to measure the data of the left and right sides of the copper recess relative to the recess of the interlayer dielectric layer, the test structure can be as follows Figure 3 As shown, the copper recess center is provided with Figure 3The left and right test copper blocks are connected in series in the horizontal direction and connected to the two terminals a and c. The upper and lower sides of the two test copper blocks are connected to two test terminals d1 and b1, d2 and b2 respectively. If the data of the upper and lower sides of the copper depression relative to the depression of the interlayer dielectric layer need to be measured, the test structure can be as follows: Figure 4 As shown, the copper depression center is provided with Figure 4 The upper and lower test copper blocks are connected in series in the vertical direction and connected to the two terminals a and c. The left and right sides of the two test copper blocks are connected to two test terminals d1 and b1, d2 and b2 respectively. Figure 3 and Figure 4 The difference between the structures is that the arrangement direction of the test copper blocks 103 is different. Figure 3 The test copper blocks 103 are arranged in one dimension along the X direction, and Figure 4 The test copper blocks 103 are arranged in one-dimensional direction along the Y direction. By testing the data of copper depression left and right and up and down relative to the depression of the interlayer dielectric layer, the position of the test copper block is changed, the depth of the copper depression at different positions is further improved, and the morphology of the copper defect is further obtained, thereby accurately simulating the depression after copper CMP.
[0049] In addition, in a further technical solution of the present invention, several test copper blocks can also be arranged in a two-dimensional direction, so as to realize the surface depression depth measurement of the test copper blocks in the two-dimensional direction, wherein the test structure includes m*n test copper blocks, and the m*n test copper blocks are spaced at a preset distance. Correspondingly, the number of the test ends is 2*(m+n), and the number of the copper blocks is (m+1)*(n+1).
[0050] Wherein, m and n are the number of test copper blocks along the x and y directions, respectively. Figure 5 FIG. 5 is a schematic diagram of a copper recess test structure provided by an embodiment of the present invention. Please refer to FIG. Figure 5 In the test structure 10 shown, the test copper blocks are arranged in two dimensions along the X and Y directions. In an example, when n=2 and m=2, the number of the test terminals is 8 and the number of the copper blocks 102 is 9. The test structure 10 can be used to measure the data of the left and right sides and the upper and lower sides of the copper depression relative to the depression of the interlayer dielectric layer. Specifically, Figure 5As shown, four test copper blocks (1035, 1036, 1037, 1038) are arranged around the center of the copper depression; the test copper blocks 1035 and 1036, and the test copper blocks 1037 and 1038 can be understood as being arranged along the X direction, and the test copper blocks 1035 and 1037, and the test copper blocks 1036 and 1038 can be understood as being arranged along the Y direction; the left and right test copper blocks 1035 and 1036 are connected in series in the horizontal direction and connected by the two endpoints d1 and b1, and the left and right test copper blocks 1037 and 1038 are connected in series in the horizontal direction and connected by the two endpoints d2 and b2; the upper and lower test copper blocks 1035 and 1037 are connected in series in the vertical direction and connected by the two endpoints a1 and c1, and the upper and lower test copper blocks 1036 and 1038 are connected in series in the vertical direction and connected by the two endpoints a2 and c2. Therefore, if it is necessary to measure the data of the left and right sides of the copper depression relative to the depression of the interlayer dielectric layer, the left and right test copper blocks 1035, 1036 and 1037, 1038 can be used for testing; if it is necessary to measure the data of the upper and lower sides of the copper depression relative to the depression of the interlayer dielectric layer, the upper and lower test copper blocks 1035, 1037 and 1036, 1038 can be used for testing. Figure 5 The test structure shown can realize data on the recess of the copper recess in two-dimensional directions on the left and right sides and the top and bottom sides relative to the recess of the interlayer dielectric layer.
[0051] In summary, the copper recessed test structure provided by the present invention can measure its electrical parameters through the test end, thereby calculating the depth of the surface recess of the test copper structure corresponding to the test end. This realizes the surface non-destructive large copper surface recess test, reduces the test cost, and improves the repeatability of the test.
[0052] Figure 7 A schematic flow chart of a method for measuring a copper recessed test structure provided by an embodiment of the present invention.
[0053] like Figure 7 As shown, the method for measuring copper recess using the copper recess test structure as described in the above embodiment of the present invention comprises the following steps:
[0054] Step S1: measuring the thickness of the interlayer dielectric layer located adjacent to the test structure; specifically, the step S1 measures the thickness of the interlayer dielectric layer using an ellipsometer.
[0055] Step S2: Obtain the resistivity ρ of the metal copper; specifically, in step S2, the resistivity ρ of the metal copper is tested by a four-probe method.
[0056] Step S3: Using the Van der Pauw method, combined with the copper resistivity ρ obtained in step S2, for the four test terminals of the test copper block at the test position, two adjacent test ends are selected for the first time to pass the first test current, and the test voltage is obtained through the remaining two test ends; the second time, two opposite test ends are selected for the second time to pass the second test current, and the test voltage is obtained through the remaining two test ends; one of the two opposite test ends in the second time and the two adjacent test ends in the first time is the same, and the thickness of the test copper block is calculated using the Van der Pauw formula.
[0057] Specifically, the Van der Pauw formula in step S3 is: Where R 1 =V 1 / I 1 , R 2 =V 2 / I 2 ; Among them, I 1 is the current applied for the first time, V 1 is the voltage measured for the first time, I 2 is the current passed in for the second time, V 2 is the voltage measured for the second time; the value of λ is calculated according to the Van der Pauw formula, and then the thickness of the test copper block is calculated according to the thickness formula: d=ρ / πλ.
[0058] Step S4: The thickness of the test copper block obtained in step S3 is subtracted from the thickness of the interlayer dielectric layer obtained in step S1 to obtain data on the recess of the position of the test copper block relative to the interlayer dielectric layer.
[0059] The technical solution provided by the present invention uses the Van der Pauw method to test the surface depression depth of the copper block in the copper depression test structure provided in the above embodiment. The electrical test method replaces the traditional AFM method, avoiding the problem of damage to the copper surface when using the AFM method in the prior art, achieving the technical effects of reducing costs and improving test repeatability; and the operation is simple.
[0060] As an example, see Figure 2 , if you need to measure Figure 2 When testing the data of the copper block depression relative to the interlayer dielectric layer in the copper depression test structure, firstly, an ellipsometer is used to measure the thickness of the interlayer dielectric layer adjacent to the test structure, and a four-probe method is used to test the resistivity ρ of the metal copper.
[0061] Secondly, place a 2*2μm 2 (or 1*1μm 2The four corners of the test copper block 103 are connected to the test ends with a width of 0.4 μm (or 0.2 μm), and the four test ends are marked as a, b, c, and d in sequence, and connected to the pads. Four large rectangular copper blocks (Cu Dummy) 102 are placed around the test copper block 103 to form a 50*50 μm 2 In this pattern, the distance between the rectangular copper blocks 102 is minimized, which can just pass the design rule checking (DRC). In this way, there is only a small oxide space between the rectangular copper blocks 102, which does not have enough resistance to polishing, so it can be approximately considered that Figure 2 The structure is similar to the depression of bulk copper after CMP, making Figure 2 The test structure can accurately simulate the depression of large copper blocks after CMP. During measurement, a current I is passed between the test terminals a and b. ab , measure the voltage V at the test terminals c and d cd ; A current I flows between the test terminals a and d ad , measure the voltage V at the test terminals b and c bc , the corresponding resistance is obtained by the voltage and the corresponding current obtained by the test, and the resistance is substituted into the Van der Pauw formula, and then the thickness of the test copper block 103 at the center position is calculated, then: the depression depth at the center position = the thickness of the interlayer dielectric layer - the thickness of the test copper block.
[0062] If it is necessary to measure the data of the left and right sides of the center of the copper depression relative to the depression of the interlayer dielectric layer, the test structure is as follows: Figure 3 First, the thickness of the interlayer dielectric layer and the resistivity ρ of the metal copper are obtained in the same way (it is assumed that these two data have been obtained in the subsequent description of this application). Secondly, when measuring the left side of the test copper block at the center position, a current I is passed through the test terminals a and b1. ab1 , measure the voltage V at the test terminals c and d1 cd1 ; Current I flows through the test terminals a and d1 ad1 , measure the voltage V at the test terminals c and b1 cb1 , the corresponding resistance is obtained by testing the voltage and the corresponding current, and the resistance is substituted into the Van der Pauw formula, and then the thickness of the copper block on the left side of the center is calculated. The depth of the depression on the left side of the center = the thickness of the interlayer dielectric layer - the thickness of the copper block. It should be noted that the test of the depression depth on the right side of the center is similar to that on the left side, and will not be repeated here.
[0063] If it is necessary to measure the data of the depression of the copper depression center above and below relative to the interlayer dielectric layer, the test structure is as follows: Figure 4 As shown, when measuring the upper side of the center point, current I flows through the test terminals a and b1. ab1, measure the voltage V at the test terminals c and d1 cd1 ; Current I flows through the test terminals a and d1 ad1 , measure the voltage V at the test terminals c and b1 cb1 , the corresponding resistance is obtained by testing the voltage and the corresponding current, and the resistance is substituted into the Van der Pauw formula, and then the thickness of the copper block on the upper side of the center position is calculated, then the depression depth on the upper side of the center position = the thickness of the interlayer dielectric layer - the thickness of the copper block. It should be noted that the test of the depression depth on the lower side of the center position is similar to that on the upper side, and will not be repeated here.
[0064] Figure 6 This is a rectangular coordinate system established with the center of the large copper block as the origin in a specific example of the present invention. Figure 6 The specific test process of the measurement method of the copper depression test structure provided by the present invention is as follows:
[0065] By using the above method and changing the position of the test copper block, the depth of the surface defects caused by copper CPM polishing at different positions can be calculated. A rectangular coordinate system can be established with the center of the large copper block as the origin, a set of position coordinates to be tested can be specified, and then the test copper blocks can be placed in the corresponding positions in the scribe path in turn. Finally, the data can be summarized to show the morphology of the depression. The depth of the depression at the boundary of the large copper block is 0.
[0066] The following is a specific example for explanation, wherein the metal layer to be measured may be the Mn layer (n=1-8), and the specific test process is as follows:
[0067] (1) The thickness of the dielectric layer on the same layer as the metal layer is measured using an ellipsometer, and the test result is Tox.
[0068] (2) The resistivity of metallic copper is tested using the four-probe method. The test result is ρ, completing the preliminary preparation work.
[0069] (3) 48*48μm 2 The center of the large copper block is used as the origin to establish a rectangular coordinate system. The coordinates of all the positions that need to be tested are as follows: Figure 6 As shown, the coordinates of C1 are (-16, 0), C2 are (-8, 0), C3 are (0, 0), C4 are (8, 0), and C5 are (16, 0); the coordinates of E3 are (0, -16), the coordinates of D3 are (0, -8), the coordinates of B3 are (0, 8), and the coordinates of A3 are (0, 16). The coordinates of the remaining points are as follows Figure 6 shown.
[0070] (4) When testing the A1 and E1 positions, Figure 4 The test copper block shown is placed in the corresponding position, and point A1 is measured first. Specifically, current I is passed through the test terminals a1 and b1. 1, the voltage V is measured at the test terminals c1 and d1 1 ; Current I flows through the test terminals a1 and d1 2 , the voltage V is measured at the test terminals c1 and b1 2 ,Depend on
[0071] R 1 =V 1 / I 1 ; R 2 =V 2 / I 2
[0072] Calculate R 1 , R 2 Then substitute into the formula
[0073]
[0074] The λ value is λ 1 , and then by
[0075] d=ρ / πλ
[0076] The value of thickness d is obtained, which is the thickness T of the test copper block at point A1. A1 , then the depth of the surface depression at point A1 is T 1 =T ox -T A1 ;
[0077] When measuring point E1, current I flows through test terminals a1 and b2. 3 , the voltage V is measured at the test terminals c1 and d2 3 ; Current I flows through the test terminals a1 and d2 4 , the voltage V is measured at the test terminals c1 and b2 4 ,Depend on
[0078] R 3 =V 3 / I 3 ; R 4 =V 4 / I 4
[0079] Calculate R 3 , R 4 Then substitute into the formula
[0080]
[0081] The λ value is λ2, and then
[0082] d=ρ / πλ
[0083] The value of thickness d is obtained, which is the thickness T of the test copper block at point E1. E1, then the depression depth T at point E1 2 =T ox -T E1
[0084] (5) When testing the A2 and E2 positions, Figure 4 The test copper block shown is placed in the corresponding position. When testing point A2, current I is passed through the test terminals a2 and b1. 1 , the voltage V is measured at the test terminals c2 and d1 1 ; Current I flows through the test terminals a2 and d1 2 , the voltage V is measured at the test terminals c2 and b1 2 , the data processing is the same as above, and the depression of point A2 is measured. When measuring point E2, the current I is passed through the test terminals a2 and b2. 3 , the voltage V is measured at the test terminals c2 and d2 3 ; Current I flows through the test terminals a2 and d2 4 , the voltage V is measured at the test terminals c2 and b2 4 , the data processing is the same as above, and the depression of point E2 is measured; according to this test process, the depth of the copper depression at An (n=3~5), En (n=3~5), Bn (n=1~5), and Dn (n=1~5) is measured in turn.
[0085] (6) When testing the C1 and C5 positions, use Figure 3 As shown in the structure, put the rectangle Cu in the corresponding position, first measure point C1, and pass the current I at the test terminals a1 and b5 5 , the voltage V is measured at the test terminals c1 and d5 5 ; Current I flows through the test terminals a1 and d5 6 , the voltage V is measured at the test terminals c1 and b5 6 ,Depend on
[0086] R 5 =V 5 / I 5 ; R 6 =V 6 / I 6
[0087] Calculate R 5 , R 6 Then substitute into the formula
[0088]
[0089] The λ value is λ3, and then
[0090] d=ρ / πλ
[0091] The value of thickness d is obtained, which is the thickness T of the test copper block at point C1. C1, then the depression depth T at point C1 3 =T ox -T C1 ;
[0092] When measuring point C5, current I flows through test terminals a5 and b5. 7 , the voltage V is measured at the test terminals c5 and d5 7 ; Current I flows through test points a5 and d5 8 , the voltage V is measured at the test terminals c5 and b5 8 ,Depend on
[0093] R 7 =V 7 / I 7 ; R 8 =V 8 / I 8
[0094] Calculate R 7 , R 8 Then substitute into the formula
[0095]
[0096] The λ value is λ4, and then
[0097] d=ρ / πλ
[0098] The value of thickness d is obtained, which is the thickness T of the test copper block at point C5. C5 , then the depression depth T at point C5 4 =T ox -T C5 The measurement methods at points C2 and C4 are the same and will not be described here.
[0099] (7) When testing the O point position, use Figure 2 The structure shown in the figure, the current I flows through the test terminals a3 and b5 01 , measure the voltage V at the test terminals c3 and d5 01 ; Current I flows through the test terminals a3 and d5 02 , measure the voltage V at the test terminals c3 and b5 02 The data processing process is as shown above, and the depression depth T at point O is calculated. o .
[0100] On the basis of the above, a three-dimensional rectangular coordinate system is established, in which the X-axis and Y-axis are the coordinates of the data points, and the Z-axis is the depth of the depression. All data are substituted into the drawing to obtain the approximate morphology of the Cu depression. It should be noted that the denser the measurement data points, the better the simulated morphology. In this way, the depression after copper CMP can be accurately simulated; since the test performed using the test structure of the present invention is a non-destructive test, the wafer after the test does not need to be scrapped, thereby reducing the test cost. And the test structure provided by the present invention can be repeatedly measured multiple times, which improves repeatability.
[0101] In summary, the copper depression test structure provided by the present invention includes at least four copper blocks of regular shape located in the interlayer dielectric layer, at least one test copper block and at least four test terminals; using at least four test terminals, the depth of the depression on the surface of the test copper block can be calculated by means of electrical measurement, avoiding the problem that the traditional AFM method of measuring surface depression easily scratches the metal surface; by changing the position of the test copper block, the measurement of the depth of the copper depression at different positions is further improved, and the morphology of the copper defect is further obtained, thereby accurately simulating the depression after copper CMP; because the test performed by the test structure of the present invention is a non-destructive test, the wafer after the test does not need to be scrapped, thereby reducing the test cost. And the test structure provided by the present invention can be repeatedly measured multiple times, which improves repeatability.
[0102] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A copper recessed test structure, the test structure being located in a dicing path of a wafer, characterized in that: include: interlayer dielectric layer; at least four regularly shaped copper blocks, at least one test copper block, and at least four test terminals; The four test ends extend from four corners of the test copper block; the four copper blocks of regular shape are each arranged between two of the test ends to surround the test copper block; The copper block, the test copper block and the test end are all embedded in the interlayer dielectric layer; The ratio of the size of the copper block to the size of the test copper block is greater than 100:1; The distance between the test end and the copper block is greater than or equal to the minimum design rule of copper process manufacturing.
2. The test structure according to claim 1, characterized in that: The test structure comprises n test copper blocks, which are spaced apart by a preset distance and arranged in a one-dimensional direction; correspondingly, the number of the test ends and the copper blocks is 2*(n+1).
3. The test structure according to claim 1, characterized in that: The test structure comprises m*n test copper blocks, which are spaced at a preset distance and arranged in two dimensions. Correspondingly, the number of the test ends is 2*(m+n), and the number of the copper blocks is (m+1)*(n+1).
4. The test structure according to any one of claims 1 to 3, characterized in that: The test copper block is located in the middle of the overall figure formed by the copper blocks.
5. The test structure according to claim 4, characterized in that: The copper block is a rectangular structure, and the overall shape of a plurality of the copper blocks after being arranged is also rectangular; the test copper block arranged between the copper blocks is a rectangular shape rotated 45 degrees relative to the adjacent copper blocks.
6. A method for measuring copper depression using the copper depression test structure as claimed in claim 1, characterized in that: The following steps are involved: Step S1: measuring the thickness of the interlayer dielectric layer located adjacent to the test structure; Step S2: Obtain the resistivity ρ of metal copper; Step S3: using the Van der Pauw method, combined with the copper resistivity ρ obtained in step S2, for the four test terminals of the test copper block at the test position, two adjacent test terminals are selected for the first time to pass the first test current, and the test voltage is obtained through the remaining two test terminals; two opposite test terminals are selected for the second time to pass the second test current, and the test voltage is obtained through the remaining two test terminals; one of the two opposite test terminals in the second time and the two adjacent test terminals in the first time is the same, and the thickness of the test copper block is calculated using the Van der Pauw formula; Step S4: The thickness of the test copper block obtained in step S3 is subtracted from the thickness of the interlayer dielectric layer obtained in step S1 to obtain data on the recess of the position of the test copper block relative to the interlayer dielectric layer.
7. The measuring method according to claim 5, characterized in that: In step S1, an ellipsometer is used to measure the thickness of the interlayer dielectric layer.
8. The measuring method according to claim 5, characterized in that: In the step S2, the resistivity ρ of the metal copper is tested by a four-probe method.
9. The measuring method according to claim 5, characterized in that: The Vanderbilt formula in step S3 is: Where R1 = V1 / I1, R2 = V2 / I2; where I1 is the current applied for the first time, V1 is the voltage measured for the first time, I2 is the current applied for the second time, and V2 is the voltage measured for the second time; the value of λ is calculated according to the Van der Pauw formula, and then according to the thickness formula: The thickness of the test copper block is calculated using d=ρ / πλ.
Citation Information
Patent Citations
Test structure and method for detecting disc trap and corrosion caused by CMP
CN101499458A
Unit and method for measuring surface indentation of polished copper wire array area
CN103474370A
Monitoring method of polishing in the semiconductor process
KR1019980066760A
Method for Measuring Dishing of Metal layer inChemical Mechanical Polishing
KR1020020068728A
Device for Measuring Leakage of Metal lines and Devicefor Sheet Resistance of the same
KR1020020094805A