Active response heat dissipation type soft driver based on shape memory effect and preparation method and application thereof
By using the combination of liquid crystal elastomer chamber and liquid heat dissipation medium in the software driver, the shape memory effect is used to achieve rapid heat dissipation and reuse, which solves the problem of low cooling speed of shape memory alloys, improves response efficiency and is suitable for thermal management applications.
Patent Information
- Application Number
- CN202411417494.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-26
AI Technical Summary
The low cooling speed of existing shape memory alloy-driven software drivers leads to low response efficiency and cannot meet the needs of rapid heat dissipation.
Using an active response heat dissipation software driver based on shape memory effect, by injecting liquid heat dissipation medium into the liquid crystal elastomer chamber, and using the bidirectional shape memory effect of the liquid crystal elastomer film and dish, it deforms when heated to squeeze the heat dissipation medium out, quickly Heat dissipation, and reuse after cooling.
It realizes the functions of rapid heat dissipation and reuse, simplifies the preparation process, the materials are lightweight, easy to industrial production, and the heat dissipation medium can be replaced as needed, suitable for the field of thermal management.
Smart Images

Figure CN119031678A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of soft drive technology, and in particular to an active response heat dissipation type soft drive based on shape memory effect and a preparation method and application thereof. Background Art
[0002] In recent years, soft actuators have attracted more and more attention due to their unlimited degrees of freedom, continuous driving, driving modes and strengths close to biological ones, and strong environmental adaptability. These advantages make them more flexible, smarter, and more biocompatible than traditional rigid components, thus attracting many researchers. Currently, soft actuators have been applied in soft robotics, bionic simulation, aerospace, and biosensing.
[0003] As a type of intelligent soft material, shape memory polymers play an important role in the field of soft actuators, and the number of soft actuators developed using shape memory polymers is gradually increasing. Currently, the most widely studied is thermotropic shape memory polymers, and liquid crystal elastomers are one of the most popular thermotropic shape memory polymers. This material uses molecules with thermosensitive reaction characteristics as "molecular switches" to achieve shape memory and recovery through phase changes caused by temperature changes, but it is mainly used to achieve flame retardant effects (CN114523685A). At the same time, there are also soft actuators that use the characteristics of shape memory alloys to integrate drive and structure, and have advantages such as high energy density and large load-to-weight ratio. However, since shape memory alloys are based on thermal drive, it takes a long time to completely cool down after heating, and the efficiency is low. Therefore, the cooling rate of shape memory alloys directly restricts the response speed of soft actuators (CN115366085A). Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides an active response heat dissipation type software driver based on shape memory effect and its preparation method and application to improve heat dissipation efficiency.
[0005] In a first aspect, the present invention provides an active response heat dissipation type soft drive based on shape memory effect, comprising a plurality of liquid crystal elastomer chambers arranged together in an array, the side walls of two adjacent liquid crystal elastomer chambers being bonded together, and each liquid crystal elastomer chamber containing a liquid heat dissipation medium; Each liquid crystal elastomer chamber includes a liquid crystal elastomer film located at the bottom, and a liquid crystal elastomer dish inverted on the liquid crystal elastomer film and tightly attached to the liquid crystal elastomer film.
[0006] Preferably, the liquid heat dissipation medium is one of oil, water, an inert liquid, a high-viscosity liquid or a liquid metal.
[0007] Preferably, the shape of the liquid crystal elastomer dish is circular, triangular or polygonal.
[0008] Preferably, the bottom thickness of the liquid crystal elastomer dish is the same as the thickness of the liquid crystal elastomer film; The side wall thickness of the liquid crystal elastomer dish is greater than the bottom thickness of the liquid crystal elastomer dish.
[0009] In a second aspect, the present invention provides a method for preparing an active response heat dissipation type soft drive based on shape memory effect, comprising the following steps: Step S11, adding the thermotropic liquid crystal monomer and the chain extender into an organic solvent, dissolving and stirring to obtain a uniformly mixed precursor solution; Step S12, adding a photoinitiator to the precursor solution, dissolving and stirring to obtain a uniformly mixed mixture to be evaporated, and transferring the mixture to be evaporated to a dispensing syringe for vacuum drying to obtain a thermotropic liquid crystal oligomeric ink; Step S13, installing the dispensing syringe filled with thermotropic liquid crystal oligomeric ink in a 3D printer, performing 3D printing and simultaneously using ultraviolet light curing to obtain a liquid crystal elastomer film and a liquid crystal elastomer dish; Step S14, pressure-assembling the liquid crystal elastomer film and the liquid crystal elastomer dish to obtain a liquid crystal elastomer chamber; Step S15, bonding a plurality of liquid crystal elastomer chambers together in an array, and injecting a liquid heat dissipation medium into each liquid crystal elastomer chamber to obtain an active response heat dissipation type soft drive based on shape memory effect.
[0010] Preferably, in step S11, the thermotropic liquid crystal monomer is 1,4-bis[4-(3-acryloxypropoxy)benzoyloxy]-2-methylbenzene, the chain extender is 2,2'-(ethylenedioxy)diethylmercaptan, and the organic solvent is at least one of dichloromethane, N,N-dimethylformamide or toluene; The molar ratio of the thermotropic liquid crystal monomer to the chain extender is 1.15:1, and the concentration of the thermotropic liquid crystal monomer in the precursor solution is 15-25%; The dissolving temperature is 10-30°C, the stirring speed is 200-400r / min, and the time is 18-24h.
[0011] Preferably, in step S12, the photoinitiator is 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone; The dissolving temperature is 10-30°C, the stirring speed is 200-400 r / min, and the time is 30-40 min; The vacuum drying temperature is 70-80°C and the time is 24-48 hours.
[0012] Preferably, in step S13, the UV curing conditions are: UV wavelength 320-395 nm, UV power 10-20 mW / cm 2 , illumination time 5 to 10 minutes; The conditions for 3D printing are: printing pressure 150-250 kPa, printing speed 5-10 mm / s, and heating temperature during printing is 80-100 °C.
[0013] Preferably, in step S14, pressure is applied to the bonding point between the liquid crystal elastomer film and the liquid crystal elastomer dish, and the pressure is maintained for 1 to 2 minutes.
[0014] In a third aspect, the present invention provides an application of an active response heat dissipation type soft driver based on shape memory effect in a soft device for thermal management.
[0015] Compared with the prior art, the present invention has the following beneficial effects: First, the active response heat dissipation software driver of the present invention has a simple preparation process, mild reaction conditions, and is also easy to industrialize; Second, the active response heat dissipation software driver of the present invention is light in material quality and fast in driving, and the liquid heat dissipation medium can be replaced as needed; Third, when the active response heat dissipation type soft drive of the present invention is heated, the liquid crystal elastomer is deformed from a permanent shape to a temporary shape, and the middle part of the liquid crystal elastomer film will bulge and become a cone, squeezing the internal space of the liquid crystal elastomer cavity, so that the liquid crystal heat dissipation medium flows from the joint of the liquid crystal elastomer and the liquid crystal elastomer dish to the outside of the liquid crystal elastomer cavity, thereby achieving rapid heat dissipation; when the active response heat dissipation type soft drive is cooled, the liquid crystal elastomer is restored from a temporary shape to a permanent shape, and the liquid crystal elastomer and the liquid crystal elastomer dish can be reassembled by pressure to reform the liquid crystal elastomer cavity, and then the liquid heat dissipation medium can be injected to form the active response heat dissipation type soft drive again, so that it can be reused; the two-way shape memory effect of the liquid crystal elastomer and the reusability make this structure have broad application prospects in the field of thermal management software devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a schematic diagram of the preparation process of the present invention.
[0017] Figure 2 Schematic diagram of the printing path of the liquid crystal elastomer film (left) and the liquid crystal elastomer dish (right) of the present invention.
[0018] Figure 3 It is a schematic diagram of pressure assembly of the liquid crystal elastomer film and the liquid crystal elastomer dish of the present invention.
[0019] Figure 4The stress-strain curve is obtained by peeling off the liquid crystal elastomer sample after pressure assembly.
[0020] Figure 5 Schematic diagram of the heat dissipation effect test method of the active response heat dissipation type software driver of the present invention (left) and the curve of the temperature change during the heat dissipation process with the heating time (right).
[0021] Figure 6 Schematic diagram (upper left) and actual picture of an actively responsive heat dissipating soft driver formed by a 4×6 liquid crystal elastomer chamber array that actively responds to high temperatures in a specific area to dissipate heat.
[0022] Figure 7 Schematic diagram (upper left) and actual picture of an actively responsive heat dissipating soft driver formed by an array of 2×12 liquid crystal elastomer chambers that actively responds to high temperatures in a specific area for heat dissipation. DETAILED DESCRIPTION
[0023] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.
[0024] Reference Figures 1 to 3 As shown, in the first aspect, the present invention provides an active response heat dissipation type soft drive based on shape memory effect, comprising a plurality of liquid crystal elastomer chambers arranged together in an array, the side walls of two adjacent liquid crystal elastomer chambers are bonded together, and each liquid crystal elastomer chamber contains a liquid heat dissipation medium; Each liquid crystal elastomer chamber includes a liquid crystal elastomer film located at the bottom, and a liquid crystal elastomer dish inverted on the liquid crystal elastomer film and tightly attached to the liquid crystal elastomer film.
[0025] It should be noted that, in the present invention, the connection between the arrays can be achieved by printing multiple liquid crystal elastomer plates and liquid crystal elastomer films together during 3D printing, or by UV curing the ink at the connection points after 3D printing.
[0026] Specifically, when the actively responsive heat dissipation type soft drive is heated, the liquid crystal elastomer is deformed from a permanent shape to a temporary shape, and the middle part of the liquid crystal elastomer film will bulge and become a cone, squeezing the internal space of the liquid crystal elastomer cavity, so that the liquid crystal heat dissipation medium flows from the joint of the liquid crystal elastomer and the liquid crystal elastomer dish to the outside of the liquid crystal elastomer cavity, thereby achieving rapid heat dissipation; when the actively responsive heat dissipation type soft drive is cooled down, the liquid crystal elastomer recovers from the temporary shape to the permanent shape, and the liquid crystal elastomer and the liquid crystal elastomer dish can be reassembled by pressure to reform the liquid crystal elastomer cavity, and then the liquid heat dissipation medium is injected (through a syringe) to form the actively responsive heat dissipation type soft drive again, so that it can be reused.
[0027] In a preferred embodiment of the present invention, the liquid heat dissipation medium is one of oil, water, inert liquid, high viscosity liquid or liquid metal. It is understandable that in other embodiments, the liquid heat dissipation medium may also be a nanofluid.
[0028] In a preferred embodiment of the present invention, the shape of the liquid crystal elastomer dish is circular, triangular or polygonal. Preferably, the height of the cone when the circle is heated is the largest (compared with the triangle, square regular polygon), so the effect of squeezing the cavity space is the best.
[0029] Preferably, the bottom thickness of the liquid crystal elastomer dish is the same as the thickness of the liquid crystal elastomer film; The side wall thickness of the liquid crystal elastomer dish is greater than the bottom thickness of the liquid crystal elastomer dish, so as to ensure that the liquid crystal elastomer cavity has sufficient strength to accommodate the liquid heat dissipation medium.
[0030] Reference Figures 1 to 3 As shown, the present invention provides a method for preparing an active response heat dissipation type soft actuator based on shape memory effect, comprising the following steps: Step S11, adding the thermotropic liquid crystal monomer and the chain extender into an organic solvent, dissolving and stirring to obtain a uniformly mixed precursor solution; In step S11, the thermotropic liquid crystal monomer is 1,4-bis[4-(3-acryloxypropoxy)benzoyloxy]-2-methylbenzene, the chain extender is 2,2'-(ethylenedioxy)diethylmercaptan, and the organic solvent is at least one of dichloromethane, N,N-dimethylformamide or toluene; The molar ratio of the thermotropic liquid crystal monomer to the chain extender is 1.15:1, and the concentration of the thermotropic liquid crystal monomer in the precursor solution is 15-25%; The dissolving temperature is 10-30°C, the stirring speed is 200-400r / min, and the time is 18-24h.
[0031] Step S12, adding a photoinitiator to the precursor solution, dissolving and stirring to obtain a uniformly mixed mixture to be evaporated, and transferring the mixture to be evaporated to a dispensing syringe for vacuum drying to obtain a thermotropic liquid crystal oligomeric ink; In step S12, the photoinitiator is 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone; The dissolving temperature is 10-30°C, the stirring speed is 200-400 r / min, and the time is 30-40 min; The vacuum drying temperature is 70-80°C and the time is 24-48 hours.
[0032] Step S13, installing the dispensing syringe filled with thermotropic liquid crystal oligomeric ink in a 3D printer, performing 3D printing and simultaneously using ultraviolet light curing to obtain a liquid crystal elastomer film and a liquid crystal elastomer dish; In step S13, the UV curing conditions are: UV wavelength 320-395 nm, UV power 10-20 mW / cm 2 , illumination time 5 to 10 minutes; The conditions for 3D printing are: printing pressure 150-250 kPa, printing speed 5-10 mm / s, and heating temperature during printing is 80-100 °C.
[0033] Specifically, in step S13, when the shape of the liquid crystal elastomer dish is circular, the movement trajectory of the printing nozzle during printing is a circular ring. After printing a circular ring, print the next concentric circle with the same center and a radius enlarged by 300-400um, and repeat the above behavior until a circular film with a radius of 5-10mm is printed. The thickness of the liquid crystal elastomer film is 100um, the bottom thickness of the liquid crystal elastomer dish is 100um, and the thickness of the outermost wall is 500-1000um. The liquid crystal elastomer film is a circular film with a radius of 5-10mm obtained by printing in a concentric circle printing path. The liquid crystal elastomer dish is a circular film with a radius of 5-10mm obtained by printing in a concentric circle printing path, and then multi-layer printing is performed on the outermost concentric circle printing path, so that the outermost layer forms a culture dish-like structure with a wall thickness of 500-1000um.
[0034] Step S14, pressure-assembling the liquid crystal elastomer film and the liquid crystal elastomer dish to obtain a liquid crystal elastomer chamber; In step S14, pressure is applied to the bonding point between the liquid crystal elastomer film and the liquid crystal elastomer dish, and the pressure is maintained for 1 to 2 minutes.
[0035] Step S15, bonding a plurality of liquid crystal elastomer chambers together in an array, and injecting a liquid heat dissipation medium into each liquid crystal elastomer chamber to obtain an active response heat dissipation type soft drive based on shape memory effect.
[0036] In a third aspect, the present invention provides an application of an active response heat dissipation type soft driver based on shape memory effect in a soft device for thermal management.
[0037] Compared with the prior art, the present invention has the following beneficial effects: First, the active response heat dissipation software driver of the present invention has a simple preparation process, mild reaction conditions, and is also easy to industrialize; Second, the active response heat dissipation software driver of the present invention is light in material quality and fast in driving, and the liquid heat dissipation medium can be replaced as needed; Third, when the active response heat dissipation type soft drive of the present invention is heated, the liquid crystal elastomer is deformed from a permanent shape to a temporary shape, and the middle part of the liquid crystal elastomer film will bulge and become a cone, squeezing the internal space of the liquid crystal elastomer cavity, so that the liquid crystal heat dissipation medium flows from the joint of the liquid crystal elastomer and the liquid crystal elastomer dish to the outside of the liquid crystal elastomer cavity, thereby achieving rapid heat dissipation; when the active response heat dissipation type soft drive is cooled, the liquid crystal elastomer is restored from a temporary shape to a permanent shape, and the liquid crystal elastomer and the liquid crystal elastomer dish can be reassembled by pressure to reform the liquid crystal elastomer cavity, and then the liquid heat dissipation medium can be injected to form the active response heat dissipation type soft drive again, so that it can be reused; the two-way shape memory effect of the liquid crystal elastomer and the reusability make this structure have broad application prospects in the field of thermal management software devices.
[0038] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. All raw materials, reagents, etc., whose manufacturers are not specified, are conventional products that can be purchased commercially. Example
[0039] (1) Thermotropic liquid crystal monomer 1,4-bis[4-(3-acryloxypropoxy)benzoyloxy]-2-methylbenzene and chain extender 2,2'-(ethylenedioxy)diethylmercaptan were weighed in molar ratios, wherein the thermotropic liquid crystal monomer was 5.886 g and the chain extender was 1.595 g.
[0040] (2) The thermotropic liquid crystal monomer 1,4-bis[4-(3-acryloxypropoxy)benzoyloxy]-2-methylbenzene and the chain extender 2,2'-(ethylenedioxy)diethylmercaptan were added to 20 ml of dichloromethane and stirred at 300 r / min at 25°C for 24 h to obtain a precursor solution with a concentration of 20%.
[0041] (3) Weigh 0.0275 g of the photoinitiator 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, add it to the precursor solution, and stir at 300 r / min at 25°C for 30 min to obtain a precursor solution containing the photoinitiator.
[0042] (4) Injecting the precursor solution containing the photoinitiator into a dispensing syringe, placing it in a vacuum drying oven at 80° C. for 48 hours to remove the dichloromethane in the precursor solution containing the photoinitiator, thereby obtaining a thermotropic liquid crystal oligomer ink.
[0043] (5) Install the dispensing syringe containing the thermotropic liquid crystal oligomer ink in an ink direct writing 3D printer, set the printing conditions to a printing pressure of 150 to 250 kPa, a printing speed of 5 to 10 mm / s, and a heating temperature of 80 to 100 °C through the G code; set the printing path to a concentric circle printing path through the G code.
[0044] (6) Start printing, use a UV lamp with a wavelength of 365nm and a power of 20mW / cm2 to irradiate during printing, and continue irradiating for 5 minutes after printing is completed. Remove the printed sample to obtain a liquid crystal elastomer film and a liquid crystal elastomer dish.
[0045] (7) Assemble the liquid crystal elastomer film and the liquid crystal elastomer dish under pressure, and fit their outermost walls together. Apply pressure only to the bonding area and maintain for 1 to 2 minutes to obtain a liquid crystal elastomer chamber.
[0046] (8) Repeat steps (6) and (7) to obtain four liquid crystal elastomer chambers. The four liquid crystal elastomer chambers are connected to form an array to obtain an active response heat dissipation soft drive.
[0047] Reference Figure 4 As shown, it can be seen from the figure that the maximum peel strength is about 1.8MPa, indicating that the bond between the two is very tight after pressure assembly.
[0048] Reference Figure 5 As shown, water is filled into four liquid crystal elastomer chambers with a syringe, the active response heat dissipation software driver is placed between two glass slides, and the bottom glass slide is heated, where T0 is the temperature of the position not affected by the active response heat dissipation software driver, T1 is the temperature of the active response heat dissipation software driver, and T2 is the temperature of the top of the active response heat dissipation software driver. It can be seen that during heating, the presence of the active response heat dissipation software driver slows down the heating rate during heating. After 3.5 minutes of continuous heating, the temperature of T0 stabilizes at about 90°C, the temperature of T1 is about 10°C lower than the temperature of T0, and the temperature of T2 is about 8°C lower than the temperature of T1, indicating that the heat dissipation effect of the active response heat dissipation software driver is excellent. Example
[0049] (1) Thermotropic liquid crystal monomer 1,4-bis[4-(3-acryloxypropoxy)benzoyloxy]-2-methylbenzene and chain extender 2,2'-(ethylenedioxy)diethylmercaptan were weighed in molar ratios, wherein the thermotropic liquid crystal monomer was 5.886 g and the chain extender was 1.595 g.
[0050] (2) The thermotropic liquid crystal monomer 1,4-bis[4-(3-acryloxypropoxy)benzoyloxy]-2-methylbenzene and the chain extender 2,2'-(ethylenedioxy)diethylmercaptan were added to 20 ml of dichloromethane and stirred at 300 r / min at 25°C for 24 h to obtain a precursor solution with a concentration of 20%.
[0051] (3) Weigh 0.0275 g of the photoinitiator 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, add it to the precursor solution, and stir at 300 r / min at 25°C for 30 min to obtain a precursor solution containing the photoinitiator.
[0052] (4) Injecting the precursor solution containing the photoinitiator into a dispensing syringe, placing it in a vacuum drying oven at 80° C. for 48 hours to remove the dichloromethane in the precursor solution containing the photoinitiator, thereby obtaining a thermotropic liquid crystal oligomer ink.
[0053] (5) Install the dispensing syringe containing the thermotropic liquid crystal oligomer ink in an ink direct writing 3D printer, set the printing conditions to a printing pressure of 150 to 250 kPa, a printing speed of 5 to 10 mm / s, and a heating temperature of 80 to 100 °C through the G code; set the printing path to a concentric circle printing path through the G code.
[0054] (6) Start printing, use a UV lamp with a wavelength of 365nm and a power of 20mW / cm2 to irradiate during printing, and continue irradiating for 5 minutes after printing is completed. Remove the printed sample to obtain a liquid crystal elastomer film and a liquid crystal elastomer dish.
[0055] (7) Assemble the liquid crystal elastomer film and the liquid crystal elastomer dish under pressure, and fit their outermost walls together. Apply pressure only to the bonding area and maintain for 1 to 2 minutes to obtain a liquid crystal elastomer chamber.
[0056] (8) Repeat steps (6) and (7) to obtain 24 liquid crystal elastomer chambers. The 24 liquid crystal elastomer chambers are connected to form a 4×6 array to obtain an active response heat dissipation soft drive.
[0057] Figure 6This is a schematic diagram (upper left) and a physical picture of the active response heat dissipation type software driver obtained in Example 2 that actively responds to heat dissipation in response to high temperatures in a specific area. Use a syringe to fill water into the active response heat dissipation type software driver, place the active response heat dissipation type software driver between two pieces of glass, use a hot air gun to heat the glass slide, and heat area 1 and area 2 to 80°C in turn. The black arrow is the direction of the hot air gun. When area 1 heats up, the part of the active response heat dissipation type software driver in area 1 responds to the high temperature and actively releases the water inside to lower the temperature; when area 2 heats up, the part of the active response heat dissipation type software driver in area 2 responds to the high temperature and actively releases the water inside to lower the temperature. Example
[0058] (1) Thermotropic liquid crystal monomer 1,4-bis[4-(3-acryloxypropoxy)benzoyloxy]-2-methylbenzene and chain extender 2,2'-(ethylenedioxy)diethylmercaptan were weighed in molar ratios, wherein the thermotropic liquid crystal monomer was 5.886 g and the chain extender was 1.595 g.
[0059] (2) The thermotropic liquid crystal monomer 1,4-bis[4-(3-acryloxypropoxy)benzoyloxy]-2-methylbenzene and the chain extender 2,2'-(ethylenedioxy)diethylmercaptan were added to 20 ml of dichloromethane and stirred at 300 r / min at 25°C for 24 h to obtain a precursor solution with a concentration of 20%.
[0060] (3) Weigh 0.0275 g of the photoinitiator 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, add it to the precursor solution, and stir at 300 r / min at 25°C for 30 min to obtain a precursor solution containing the photoinitiator.
[0061] (4) Injecting the precursor solution containing the photoinitiator into a dispensing syringe, placing it in a vacuum drying oven at 80° C. for 48 hours to remove the dichloromethane in the precursor solution containing the photoinitiator, thereby obtaining a thermotropic liquid crystal oligomer ink.
[0062] (5) Install the dispensing syringe containing the thermotropic liquid crystal oligomer ink in an ink direct writing 3D printer, set the printing conditions to a printing pressure of 150 to 250 kPa, a printing speed of 5 to 10 mm / s, and a heating temperature of 80 to 100 °C through the G code; set the printing path to a concentric circle printing path through the G code.
[0063] (6) Start printing, use a UV lamp with a wavelength of 365nm and a power of 20mW / cm2 to irradiate during printing, and continue irradiating for 5 minutes after printing is completed. Remove the printed sample to obtain a liquid crystal elastomer film and a liquid crystal elastomer dish.
[0064] (7) Assemble the liquid crystal elastomer film and the liquid crystal elastomer dish under pressure, and fit their outermost walls together. Apply pressure only to the bonding area and maintain for 1 to 2 minutes to obtain a liquid crystal elastomer chamber.
[0065] (8) Repeat steps (6) and (7) to obtain 24 liquid crystal elastomer chambers. The 24 liquid crystal elastomer chambers are connected to form a 2×12 array to obtain an active response heat dissipation soft drive.
[0066] Figure 7 The schematic diagram (above 1) and the actual picture of the active response heat dissipation type software driver obtained in Example 3 for active response heat dissipation in response to high temperature in a specific area. Use a syringe to fill water into the active response heat dissipation type software driver, place the active response heat dissipation type software driver between two pieces of glass, use a hot air gun to heat the glass slide, and heat only the area shown by the dotted line in the figure each time, and heat to 80°C. The black arrow is the direction of the hot air gun. Then move the hot air gun in the direction of the white arrow. In the process of the hot air gun moving from right to left, the part of the active response heat dissipation type software driver in the heated area responds to the high temperature and actively releases the water inside to lower the temperature.
[0067] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.
Claims
1. An active response heat dissipation type soft driver based on shape memory effect, characterized in that: It comprises a plurality of liquid crystal elastomer chambers arranged in an array, the side walls of two adjacent liquid crystal elastomer chambers are bonded together, and each liquid crystal elastomer chamber contains a liquid heat dissipation medium; Each liquid crystal elastomer chamber includes a liquid crystal elastomer film located at the bottom, and a liquid crystal elastomer dish inverted on the liquid crystal elastomer film and tightly attached to the liquid crystal elastomer film.
2. The active response heat dissipation type soft driver based on shape memory effect according to claim 1, characterized in that: The liquid heat dissipation medium is one of oil, water, inert liquid, high viscosity liquid or liquid metal.
3. The active response heat dissipation type software driver based on shape memory effect according to claim 1, characterized in that: The shape of the liquid crystal elastomer dish is circular, triangular or polygonal.
4. The active response heat dissipation type software driver based on shape memory effect according to claim 1, characterized in that: The thickness of the bottom of the liquid crystal elastomer dish is the same as the thickness of the liquid crystal elastomer film; The side wall thickness of the liquid crystal elastomer dish is greater than the bottom thickness of the liquid crystal elastomer dish.
5. A method for preparing an active response heat dissipation type soft driver based on shape memory effect, characterized in that: The following steps are involved: Step S11, adding the thermotropic liquid crystal monomer and the chain extender into an organic solvent, dissolving and stirring to obtain a uniformly mixed precursor solution; Step S12, adding a photoinitiator to the precursor solution, dissolving and stirring to obtain a uniformly mixed mixture to be evaporated, and transferring the mixture to be evaporated to a dispensing syringe for vacuum drying to obtain a thermotropic liquid crystal oligomeric ink; Step S13, installing the dispensing syringe filled with thermotropic liquid crystal oligomeric ink in a 3D printer, performing 3D printing and simultaneously using ultraviolet light curing to obtain a liquid crystal elastomer film and a liquid crystal elastomer dish; Step S14, pressure-assembling the liquid crystal elastomer film and the liquid crystal elastomer dish to obtain a liquid crystal elastomer chamber; Step S15, bonding a plurality of liquid crystal elastomer chambers together in an array, and injecting a liquid heat dissipation medium into each liquid crystal elastomer chamber to obtain an active response heat dissipation type soft drive based on shape memory effect.
6. The active response heat dissipation type software driver based on shape memory effect according to claim 5, characterized in that: In step S11, the thermotropic liquid crystal monomer is 1,4-bis[4-(3-acryloxypropoxy)benzoyloxy]-2-methylbenzene, the chain extender is 2,2'-(ethylenedioxy)diethylmercaptan, and the organic solvent is at least one of dichloromethane, N,N-dimethylformamide or toluene; The molar ratio of the thermotropic liquid crystal monomer to the chain extender is 1.15:1, and the concentration of the thermotropic liquid crystal monomer in the precursor solution is 15-25%; The dissolving temperature is 10-30°C, the stirring speed is 200-400r / min, and the time is 18-24h.
7. The active response heat dissipation type software driver based on shape memory effect according to claim 5, characterized in that: In step S12, the photoinitiator is 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone; The dissolving temperature is 10-30°C, the stirring speed is 200-400 r / min, and the time is 30-40 min; The vacuum drying temperature is 70-80°C and the time is 24-48 hours.
8. The active response heat dissipation type software driver based on shape memory effect according to claim 5, characterized in that: In step S13, the UV curing conditions are: UV wavelength 320-395 nm, UV power 10-20 mW / cm 2 , illumination time 5 to 10 minutes; The conditions for 3D printing are: printing pressure 150-250 kPa, printing speed 5-10 mm / s, and heating temperature during printing is 80-100 °C.
9. The active response heat dissipation type software driver based on shape memory effect according to claim 5, characterized in that: In step S14, pressure is applied to the bonding point between the liquid crystal elastomer film and the liquid crystal elastomer dish, and the pressure is maintained for 1 to 2 minutes.
10. Application of the active response heat dissipation software driver based on shape memory effect according to any one of claims 1 to 4 in a software device for thermal management.