Method for manufacturing semiconductor device and semiconductor device

By setting a barrier metal layer between the electrode and the insulating film of the semiconductor device and using organic materials, the problem of interface migration between the electrode and the insulating film is solved, the connection reliability and stability of the semiconductor device are improved, and the fine wiring is realized structure.

CN119032415APending Publication Date: 2024-11-26RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034012.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-28
Filing Date
2023-02-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In a three-dimensionally mounted semiconductor device, the interface between the electrode and the insulating film is prone to migration, resulting in poor connection and peeling, which affects the reliability and stability of the device.

Method used

By providing a barrier metal layer between the electrode and the insulating film, the adhesive strength is improved, and organic materials are used in the insulating film to absorb foreign matter and reduce connection failures, stable bonding between the electrode and the insulating film is ensured.

Benefits of technology

The interface migration and peeling between the electrode and the insulating film are effectively suppressed, the connection reliability and stability of the semiconductor device are improved, and the fine wiring structure is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119032415A_ABST
    Figure CN119032415A_ABST
Patent Text Reader

Abstract

A method for manufacturing a semiconductor device includes: a step for preparing a first substrate having a first support substrate, a first insulating film, and a first electrode provided in a first recess of the first insulating film; a step for preparing a second substrate having a second support substrate, a second insulating film, and a second electrode provided in a second recess of the second insulating film; a step for bonding the first insulating film of the first substrate and the second insulating film of the second substrate; and a step for joining the first electrode of the first substrate and the second electrode of the second substrate. The first insulating film includes an organic insulating film. The first electrode includes: a first electrode body provided in the first recess; a first barrier metal provided on at least one of an inner surface and a bottom surface of the first recess and covering a portion of the first electrode body; and a second barrier metal covering the surface of the first electrode main body on the opening side of the first recess. The adhesive strength between the first insulating film and the first barrier metal is 30 MPa or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a semiconductor device and a semiconductor device. Background Art

[0002] In recent years, three-dimensional packaging has been studied to improve the integration of large-scale collective circuits. Patent Document 1 and Non-Patent Document 1 disclose an example of three-dimensional packaging of semiconductor chips.

[0003] Previous technical literature

[0004] Patent Literature

[0005] Patent Document 1: U.S. Patent Application Publication No. 2021 / 002815

[0006] Non-patent literature

[0007] Non-patent document 1: FCChen et al., "Systemon Integrated Chips (SoIC TM) for 3DHeterogeneous Integration", 2019IEEE 69th Electronic Components and Technology Conference (ECTC), p.594-599 (2019) Summary of the invention

[0008] Technical issues to be solved by the invention

[0009] When manufacturing semiconductor devices by three-dimensional mounting, hybrid bonding technology is being studied to miniaturize the wiring between devices. Figure 7 As shown in (b), when hybrid bonding is performed, a slight positional offset S may occur when the terminal electrodes (the first electrode 113 and the second electrode 123) are bonded to each other. This positional offset S may be caused by, for example, the miniaturization of the terminal electrodes themselves or the difference in thermal expansion coefficients caused by heating during bonding. When this positional offset S occurs in a semiconductor device, copper or the like constituting the terminal electrodes dissolves in the resin constituting the insulating film (the first insulating film 112 and the second insulating film 122), which may cause migration at the interface between the electrode or the copper or the like and the insulating film.

[0010] An object of the present invention is to provide a method for manufacturing a semiconductor device and a semiconductor device capable of suppressing migration at the interface between an electrode and an insulating film.

[0011] Means for solving technical problems

[0012] [1] As one aspect of the present invention, it relates to a method for manufacturing a semiconductor device. The method for manufacturing a semiconductor device includes: a) a process of preparing a first substrate, the first substrate having a first supporting substrate, a first insulating film disposed on the first supporting substrate, and a first electrode disposed in a first recess of the first insulating film and exposed from a first surface side of the first insulating film; b) a process of preparing a second substrate, the second substrate having a second supporting substrate, a second insulating film disposed on the second supporting substrate, and a second electrode disposed in a second recess of the second insulating film and exposed from a second surface side of the second insulating film; c) a process of bonding the first insulating film of the first substrate and the second insulating film of the second substrate; and d) a process of bonding the first electrode of the first substrate and the second electrode of the second substrate. The first insulating film includes an organic insulating film. The first electrode includes: a first electrode body disposed in a first recess; a first barrier metal disposed on at least one of an inner surface and a bottom surface of the first recess and covering a portion of the first electrode body; and a second barrier metal covering a surface of the first electrode body on an opening side of the first recess. The bonding strength between the first insulating film and the first barrier metal is 30 MPa or more.

[0013] In the manufacturing method of the semiconductor device, the first electrode provided on the first insulating film includes: a first barrier metal covering a part of the first electrode body; and a second barrier metal covering the surface of the first electrode body on the opening side of the first recess. At this time, the dissolution of the first electrode body, which is mostly formed of a material that is easily dissolved, such as copper, is suppressed by the first barrier metal and the second barrier metal. Thus, even if a positional offset occurs between the first electrode and the second electrode at any stage, the migration of the interface between the first electrode and the first insulating film can be suppressed. In addition, the positional offset mentioned here also includes extremely small positional offsets as long as there is a position where migration may occur. The same is true in the following cases. In addition, although the electrode material such as copper is weakly bonded to the resin constituting the insulating film (organic insulating film) and sometimes causes peeling, it is possible to suppress such peeling by providing the first barrier metal on at least one of the inner surface and the bottom surface of the first recess of the first insulating film to cover a part of the first electrode body, and the bonding strength between the first insulating film and the first barrier metal is 30 MPa or more.

[0014] Furthermore, in the method for manufacturing the semiconductor device, the first insulating film includes an organic insulating film. At this time, foreign matter (fragments) attached to the surface of the first substrate can be absorbed into the insulating film by a relatively soft material, namely an organic material, to reduce the poor connection between the first substrate and the second substrate. The organic insulating material contained in the insulating film can be polyimide, a polyimide precursor, polyamide-imide, benzocyclobutene (BCB), polybenzoxazole (PBO) or a PBO precursor. Since these materials are soluble in liquid or solvent, it is easy to make an insulating film by, for example, spin coating, and it is easy to form a thin film. Furthermore, since these materials have high heat resistance, they can withstand the high temperature when joining the first substrate and the second substrate, and the first substrate and the second substrate can be joined more reliably. In addition, in the first insulating film, a part can be formed by an inorganic insulating film, and another part (for example, the surface side) can be formed by an organic insulating film.

[0015] [2] In the method for manufacturing a semiconductor device of [1], the bonding strength between the first insulating film and the first barrier metal is more preferably 40 MPa or more. In this case, the first barrier metal can further suppress the peeling between the electrode body composed of copper or the like and the organic insulating film. In addition, the bonding strength between the first insulating film and the first barrier metal can be 50 MPa or more.

[0016] [3] In the above-mentioned method for manufacturing a semiconductor device, the step of a) preparing a first substrate may include: a1) forming a first insulating film on a first supporting substrate; a2) forming at least one first recess in the first insulating film; a3) forming a first barrier metal on the inner surface and bottom surface of the first recess; a4) forming a first electrode body in the first recess and in a region surrounded by the first barrier metal; and a5) forming a second barrier metal on the surface of the first electrode body. Furthermore, the step of b) preparing a second substrate may include: b1) forming a second insulating film on a second supporting substrate; b2) forming at least one second recess in the second insulating film; b3) forming a third barrier metal on the inner surface and bottom surface of the second recess; b4) forming a second electrode body in the second recess and in a region surrounded by the third barrier metal; and b5) forming a fourth barrier metal on the surface of the second electrode body.

[0017] [4] In the method for manufacturing a semiconductor device of [3] above, in the step of forming the first barrier metal, the first barrier metal may be formed in the first recessed portion of the first insulating film by electroless plating. In this case, the bonding strength between the first insulating film and the first barrier metal may be easily improved.

[0018] [5] In the method for manufacturing a semiconductor device of [4] above, in the step of forming the first electrode body, the first barrier metal is used as a power supply layer and the first electrode body can be formed by electroplating. In this case, the bonding strength between the first barrier metal and the first electrode body can also be improved.

[0019] [6] In the method for manufacturing a semiconductor device according to any one of [3] to [5] above, a4) in the step of forming the first electrode body, a conductive material may be arranged on the first barrier metal and the first insulating film in the first recess so as to bury the first recess, and the first electrode body may be formed by grinding the arranged conductive material. Also, b4) in the step of forming the second electrode body, a conductive material may be arranged on the third barrier metal and the second insulating film in the second recess so as to bury the second recess, and the second electrode body may be formed by grinding the arranged conductive material.

[0020] [7] In the method for manufacturing a semiconductor device of [6] above, a4) in the process of forming the first electrode body, the first insulating film may be ground after grinding the conductive material, and b4) in the process of forming the second electrode body, the second insulating film may be further ground after grinding the conductive material. The surface roughness of the ground first insulating film and the second insulating film may be 0.1 μm or less. By making the surface roughness of the first insulating film and the second insulating film 0.1 μm or less, the bonding strength when the first insulating film and the second insulating film are bonded together can be improved. In addition, the surface roughness used here is the arithmetic mean roughness Ra measured using a laser microscope at a magnification of 20 times, and is the arithmetic mean roughness Ra specified in JIS B 0601 2001.

[0021] [8] In the method for manufacturing a semiconductor device of [6] or [7] above, a5) in the step of forming the second barrier metal, the second barrier metal may be formed to cover the surface of the first electrode body after grinding the conductive material, and b5) in the step of forming the fourth barrier metal, the fourth barrier metal may be formed to cover the surface of the second electrode body after grinding the conductive material. In this case, the bonding strength between the first electrode body and the second barrier metal and the bonding strength between the second electrode body and the fourth barrier metal can be improved.

[0022] [9] In the method for manufacturing a semiconductor device according to any one of [3] to [8] above, a) in the step of preparing the first substrate, before the step of forming the second barrier metal, a step of modifying the surface of the first electrode body by at least one of ultraviolet irradiation, electron beam irradiation, ozone water treatment, corona discharge treatment and plasma treatment is included. In this case, the bonding strength of the second barrier metal to the first electrode body can be improved, and migration can be suppressed by suppressing peeling of the second barrier metal. In addition, b) in the step of preparing the second substrate, the surface of the second electrode body can be subjected to the same treatment.

[0023]

[10] In the method for manufacturing a semiconductor device according to any one of [1] to [9] above, the entire first electrode body is preferably covered by the first barrier metal and the second barrier metal. In this case, migration of the interface between the first electrode and the first insulating film can be more reliably suppressed. Furthermore, the entire second electrode body is preferably covered by the third barrier metal and the fourth barrier metal. In this case, migration of the interface between the second electrode and the second insulating film can be more reliably suppressed.

[0024]

[11] In the method for manufacturing a semiconductor device according to any one of [1] to

[10] above, the thickness of the second barrier metal before the first electrode and the second electrode are bonded can be 1 μm or less, and the thickness of the fourth barrier metal before the first electrode and the second electrode are bonded can be 1 μm or less. In this case, the terminal electrode can be miniaturized more reliably.

[0025]

[12] In the method for manufacturing a semiconductor device of any one of [1] to

[11] above, the second insulating film may include an organic insulating film, and the second electrode may include: a second electrode body disposed in the second recess; a third barrier metal covering a portion of the second electrode body disposed on at least one of the inner surface and the bottom surface of the second recess; and a fourth barrier metal covering the surface of the second electrode body on the opening side of the second recess. In this manufacturing method, the bonding strength between the second insulating film and the third barrier metal is preferably 30 MPa or more. At this time, the dissolution of the second electrode body, which is mostly formed of an easily dissolving material such as copper, is suppressed by the third barrier metal and the fourth barrier metal. Thus, even if a positional shift occurs between the first electrode and the second electrode at any stage, the migration of the interface between the second electrode and the second insulating film can be suppressed. Furthermore, although the electrode material such as copper is weakly bonded to the resin constituting the insulating film (organic insulating film) and sometimes causes peeling, such peeling can be suppressed by providing the third barrier metal on at least one of the inner surface and the bottom surface of the second concave portion of the second insulating film to cover a portion of the second electrode body, and the bonding strength between the second insulating film and the third barrier metal is 30 MPa or more. In addition, similarly to the case of the first insulating film, the second insulating film can include an organic insulating film to absorb foreign matter and reduce poor connection. In addition, the bonding strength between the second insulating film and the third barrier metal can be 40 MPa or more, or 50 MPa or more.

[0026]

[13] In the method for manufacturing a semiconductor device of

[12] above, the first electrode may be formed in such a manner that the surface of the second barrier metal is recessed inwardly relative to the first surface of the first insulating film, and the second electrode may be formed in such a manner that the surface of the fourth barrier metal is protruded outwardly relative to the second surface of the second insulating film. In this case, c) in the step of bonding the first insulating film and the second insulating film, the protruding portion of the fourth barrier metal is preferably embedded in the recessed region of the second barrier metal. By such a concave-convex structure, the first substrate and the second substrate can be more reliably aligned to prevent positional deviation, thereby further suppressing the migration of the interface between the electrode and the insulating film.

[0027]

[14] In the method for manufacturing a semiconductor device according to any one of [1] to

[13] above, at least one semiconductor element may be arranged in the first supporting substrate or on the surface of the first supporting substrate opposite to the surface on which the first insulating film is formed. Furthermore, at least one semiconductor element may be arranged in the second supporting substrate or on the surface of the second supporting substrate opposite to the surface on which the second insulating film is formed.

[0028]

[15] In the method for manufacturing a semiconductor device according to any one of [1] to

[14] , when the first electrode and the second electrode are bonded, the second barrier metal and the fourth barrier metal may be bonded. In this case, even if positional displacement occurs between the first electrode and the second electrode, a portion of at least one of the second barrier metal and the fourth barrier metal is bonded to the resin to prevent the first electrode body and the second electrode body from being bonded to the resin. Thus, migration of the interface between the first electrode and the first insulating film and the interface between the second electrode and the second insulating film can be more reliably suppressed.

[0029]

[16] In the method for manufacturing a semiconductor device according to any one of [1] to

[15] above, the second barrier metal and the fourth barrier metal preferably include at least one selected from titanium, nickel, palladium, chromium, tantalum, tungsten, cobalt and gold. More preferably, the second barrier metal and the fourth barrier metal include at least one selected from nickel, cobalt and tungsten. Since these materials have a low ionization tendency, they have a high barrier capability. By including the second barrier metal and the fourth barrier metal in such a material with a high barrier capability, migration at the interface between the first electrode and the first insulating film and at the interface between the second electrode and the second insulating film can be more reliably suppressed.

[0030]

[17] In the method for manufacturing a semiconductor device according to any one of [1] to

[16] , the first recess and the second recess preferably have an opening diameter or opening width of 5 μm or more and 50 μm or less. According to this method for manufacturing a semiconductor device, even when a terminal electrode or a wiring electrode is formed in such a fine recess, migration can be suppressed, so that a semiconductor device having fine wiring can be manufactured.

[0031]

[18] In the method for manufacturing a semiconductor device according to any one of [1] to

[17] , at least one of the first insulating film and the second insulating film may partially include an inorganic insulating film. When the insulating film includes an inorganic insulating film, it is easy to miniaturize a recessed portion for forming a terminal electrode, etc., so that a semiconductor device having finer wiring can be manufactured. Furthermore, since it is easy to firmly bond inorganic materials to each other, the connection reliability of the semiconductor device can be improved by improving the bonding strength between the first substrate and the second substrate.

[0032]

[19] In the method for manufacturing a semiconductor device according to any one of [1] to

[18] , the second barrier metal and the fourth barrier metal may be formed by electroplating. In this case, it is possible to easily manufacture thinner and finer barrier metals.

[0033]

[20] As another aspect of the present invention, it relates to a semiconductor device. The semiconductor device includes a first substrate and a second substrate. The first substrate includes a first supporting substrate, a first insulating film disposed on the first supporting substrate, and a first electrode disposed in a first recess of the first insulating film and exposed from a first surface side of the first insulating film. The second substrate includes a second supporting substrate, a second insulating film disposed on the second supporting substrate, and a second electrode disposed in a second recess of the second insulating film and exposed from a second surface side of the second insulating film. In the semiconductor device, the first insulating film includes an organic insulating film, the first insulating film and the second insulating film are bonded, and the first electrode and the second electrode are bonded. The first electrode includes: a first electrode body disposed in the first recess; a first barrier metal disposed on at least one of the inner surface and the bottom surface of the first recess and covering a portion of the first electrode body; and a second barrier metal covering the surface of the first electrode body on the opening side of the first recess. The bonding strength between the first insulating film and the first barrier metal is 30 MPa or more.

[0034] In the semiconductor device, the first electrode provided on the first insulating film has: a first barrier metal covering a portion of the first electrode body; and a second barrier metal covering the surface of the first electrode body on the opening side of the first recess. At this time, the dissolution of the first electrode body, which is mostly formed of a material that is easily dissolved, such as copper, is suppressed by the first barrier metal and the second barrier metal. Thus, the migration of the interface between the first electrode and the first insulating film can be suppressed. In addition, although the electrode material such as copper is weakly bonded to the resin constituting the insulating film (organic insulating film) and sometimes causes peeling, it is also possible to suppress such peeling by providing the first barrier metal on at least one of the inner surface and the bottom surface of the first recess of the first insulating film to cover a portion of the first electrode body, and the bonding strength between the first insulating film and the first barrier metal is 30 MPa or more. In addition, the bonding strength between the first insulating film and the first barrier metal can be 40 MPa or more, or 50 MPa or more.

[0035] In the semiconductor device, the second insulating film includes an organic insulating film, and the second electrode may include: a second electrode body disposed in the second recess; a third barrier metal covering a portion of the second electrode body disposed on at least one of the inner surface and the bottom surface of the second recess; and a fourth barrier metal covering the surface of the second electrode body on the opening side of the second recess. The bonding strength between the second insulating film and the third barrier metal is 30 MPa or more. At this time, the dissolution of the second electrode body, which is mostly formed of a material that is easily eluted, such as copper, is suppressed by the third barrier metal and the fourth barrier metal. Thus, the migration of the interface between the second electrode and the second insulating film can be suppressed. In addition, although the electrode material such as copper is weakly bonded to the resin constituting the insulating film (organic insulating film) and sometimes causes peeling, it is also possible to suppress such peeling by disposing the third barrier metal on at least one of the inner surface and the bottom surface of the second recess of the second insulating film to cover a portion of the second electrode body, and the bonding strength between the second insulating film and the third barrier metal is 30 MPa or more. In addition, the bonding strength between the second insulating film and the third barrier metal may be 40 MPa or more, or 50 MPa or more.

[0036] Effects of the Invention

[0037] According to the present invention, migration at the interface between an electrode and an insulating film can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a cross-sectional view showing an example of a semiconductor device manufactured by a method according to an embodiment of the present invention.

[0039] Figure 2 It is a magnified representation Figure 1 2 is a cross-sectional view of a junction A of electrodes in a semiconductor device shown in FIG.

[0040] Figure 3 It is used to illustrate the manufacturing Figure 1 0 is a cross-sectional view of a method for manufacturing a semiconductor device shown in , and shows an example of a process for manufacturing a first substrate and a second substrate.

[0041] Figure 4 It is a magnified representation Figure 3 (d) is a cross-sectional view of region B shown.

[0042] Figure 5 It is used to illustrate the manufacturing Figure 1 A cross-sectional view of a semiconductor device method is shown, followed by Figure 3 The process of bonding the first substrate and the second substrate is shown as an example.

[0043] Figure 6 It means in Figure 5 A cross-sectional view of an example in which positional deviation occurs in the process shown in FIG.

[0044] Figure 7 (a) is a cross-sectional view showing a case where positional deviation occurs at a junction of a semiconductor device manufactured by the method of this embodiment. Figure 7 (b) is a cross-sectional view showing a case where positional deviation occurs at a junction of a semiconductor device manufactured by the method of the comparative example.

[0045] Figure 8 is a cross-sectional view for explaining a first variation of the method for manufacturing a semiconductor device according to the present embodiment. Figure 8 (a) is a cross-sectional view before bonding electrodes. Figure 8 (b) is a cross-sectional view after the electrodes are bonded.

[0046] Fig. 9 It is a cross-sectional view for explaining a second modified example of the method for manufacturing the semiconductor device according to the present embodiment.

[0047] Fig.10 It is a cross-sectional view for explaining a third modified example of the method for manufacturing the semiconductor device according to the present embodiment. DETAILED DESCRIPTION

[0048] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. In the following description, the same or equivalent parts are marked with the same element symbols, and repeated descriptions are omitted. In addition, regarding positional relationships such as up, down, left, and right, unless otherwise specified, they are assumed to be based on the positional relationships shown in the accompanying drawings. In addition, the dimensional ratios of the accompanying drawings are not limited to the ratios shown in the drawings.

[0049] In this specification, when viewed from above, the term "layer" includes not only structures of shapes formed on the entire surface, but also structures of shapes formed on a portion of the surface. Furthermore, in this specification, the term "process" is not only used as an independent process, but is also included in this term as long as the desired effect of the process can be achieved even when it cannot be clearly distinguished from other processes. Furthermore, a numerical range expressed using "to" indicates a range that includes the numerical values ​​recorded before and after "to" as the minimum and maximum values, respectively.

[0050] (Structure of Semiconductor Device)

[0051] Figure 1 It is a cross-sectional view showing an example of a semiconductor device manufactured by a method according to an embodiment of the present invention. Figure 2 It is a magnified representation Figure 1 FIG. 1 is a cross-sectional view of a junction A of electrodes in a semiconductor device shown in FIG. The semiconductor device 1 is an example of a semiconductor package. Figure 1 and Figure 2As shown, the semiconductor device 1 includes a first substrate 10 and a second substrate 20. In the semiconductor device 1, the first substrate 10 and the second substrate 20 are bonded together. The first substrate 10 may include a semiconductor chip 30 (semiconductor element), and the second substrate 20 may include a semiconductor chip 40 (semiconductor element). The semiconductor chip 30 may be arranged on the surface ( Figure 1 The semiconductor chip 40 may be disposed on the surface of the second substrate 20 opposite to the first substrate 10 ( Figure 1 The semiconductor chips 30 and 40 may be, for example, LSI (Large scale Integrated Circuit) chips, CMOS (Complementary Metal Oxide Semiconductor) sensors, memories, and other semiconductor chips. The semiconductor chips 30 and 40 may be other types of semiconductor chips.

[0052] The first substrate 10 includes a first supporting substrate 11, a first insulating film 12, and a plurality of first electrodes 13. The first insulating film 12 is provided on the first supporting substrate 11. Each first electrode 13 is provided in a first recess 14 formed in the first insulating film 12 and is formed so as to be exposed from a first surface 12a of the first insulating film 12.

[0053] The first support substrate 11 is not particularly limited, and may be, for example, a silicon plate, a glass plate, a SUS plate, a glass cloth-containing substrate, a semiconductor element sealing resin, etc. The first support substrate 11 is preferably a high-rigidity substrate. The thickness of the first support substrate 11 is preferably, for example, in the range of 0.2 mm to 2.0 mm. By having a thickness of 0.2 mm or more, the operability of the first support substrate 11 can be improved. Furthermore, by having a thickness of 2.0 mm or less, the material cost can be reduced, and the semiconductor device 1 can be thinned. The shape when the first support substrate 11 is viewed from above may be any one of a wafer shape (circular plate shape) and a panel shape (rectangular shape). The size (dimensions) of the first support substrate 11 is not particularly limited, and may be, for example, a wafer shape of 200 mm in diameter, 300 mm in diameter, or 450 mm in diameter, or a rectangular panel with a side of 300 mm to 700 mm. In addition, the semiconductor chip 30 may be disposed on the inner side of the first support substrate 11 or on the surface of the first support substrate 11 opposite to the second substrate 20 ( Figure 1 lower surface).

[0054] The first insulating film 12 is formed of an organic insulating material. The first insulating film 12 may partially contain an inorganic insulating material. The organic insulating material forming the first insulating film 12 is, for example, a photosensitive organic insulating material or a thermosetting organic insulating material. The inorganic insulating material forming the first insulating film 12 is, for example, a silicon-containing material such as silicon nitride (SiN), silicon dioxide (SiO2) or silicon oxynitride (SiON). More specifically, the organic insulating material forming the first insulating film 12 may be, for example, polyimide, a polyimide precursor, polyamide-imide, benzocyclobutene (BCB), polybenzoxazole (PBO) or a PBO precursor. Since these materials are soluble in liquid or solvent, it is easy to make an insulating film by, for example, spin coating, and it is easy to form a thin film. In addition, since these materials have high heat resistance, they can withstand the high temperature when the first substrate 10 and the second substrate 20 are bonded, and the first substrate 10 and the second substrate 20 can be bonded more reliably. The organic insulating material forming the first insulating film 12 may be a liquid or film-like material, and is preferably a film-like material from the viewpoint of film thickness flatness and cost. The first insulating film 12 may preferably contain a filler in the organic insulating material, and the average particle size of the filler contained in the insulating material is 500 nm or less. By containing such a filler, a fine groove structure can be easily formed in the first insulating film 12. In addition, the first insulating film 12 may not contain a filler. The particle size of the filler can be measured using a laser diffraction particle size distribution measurement method.

[0055] When the first insulating film 12 is formed by laminating a film-like organic insulating material on the first supporting substrate 11, it is preferably laminated in a low temperature process, and therefore preferably a photosensitive organic insulating film that can be laminated at 40°C to 120°C. Since the temperature at which the photosensitive insulating film used for the first insulating film 12 can be laminated is 40°C or higher, the viscosity can be reduced at room temperature and it is easy to handle. By setting the temperature at which the photosensitive insulating film used for the first insulating film 12 can be laminated to 120°C or lower, the warping of the laminated photosensitive insulating film can be reduced. From the viewpoint of suppressing warping, the thermal expansion coefficient of the organic insulating material used for the first insulating film 12 after curing is preferably 80 ppm / °C or lower, and more preferably 70 ppm / °C or lower from the viewpoint of obtaining high reliability. From the viewpoint of obtaining stress relaxation properties and high-definition patterns, the thermal expansion coefficient of the insulating material used for the first insulating film 12 after curing is preferably 20 ppm / °C or higher.

[0056] The thickness of the first insulating film 12 is preferably 10 μm or less, more preferably 5 μm or less, and further preferably 3 μm or less. By setting the thickness of the first insulating film 12 to such a thickness, the first recess 14 formed in the first insulating film 12 can be miniaturized. From the viewpoint of ensuring electrical reliability, the thickness of the first insulating film 12 is preferably 1 μm or more.

[0057] The first electrode 13 is an electrode formed in the first insulating film 12, and has a first electrode body 13a, a first barrier metal 13b and a second barrier metal 13c. The first electrode 13 may be a terminal electrode such as a bump, or may be a wiring electrode. The first electrode body 13a is disposed in the first recess 14 formed in the first insulating film 12, and is formed of, for example, a material having high conductivity such as copper, aluminum or silver. The first barrier metal 13b is disposed on the inner surface 14a and the bottom surface 14b of the first recess 14, covering the side surface and the bottom surface of the first electrode body 13a. The thickness of the first barrier metal 13b is, for example, in the range of 0.1 μm to 0.8 μm. The bonding strength between the first insulating film 12 and the first barrier metal 13b is 30 MPa or more. The bonding strength between the first insulating film 12 and the first barrier metal 13b is preferably 40 MPa or more, and more preferably 50 MPa or more. The second barrier metal 13c covers the surface of the first electrode body 13a on the opening side of the first recess 14. The thickness of the second barrier metal 13c is, for example, in the range of 0.1 μm to 0.8 μm, and is 1 μm or less before being bonded to the second electrode. The first electrode body 13a is completely covered by the first barrier metal 13b and the second barrier metal 13c.

[0058] The first barrier metal 13b and the second barrier metal 13c are used to prevent the first electrode body 13a from being dissolved into the resin formed by the easily ionized material, and are composed of a conductive material with a low ionization tendency. The first barrier metal 13b and the second barrier metal 13c are composed of, for example, at least one selected from titanium, nickel, palladium, chromium, tantalum, tungsten, cobalt and gold. The first barrier metal 13b and the second barrier metal 13c are preferably electroplated films (for example, electroless plating films), for example, preferably nickel electroplated films, palladium electroplated films, cobalt electroplated films, gold electroplated films or alloy electroplated films containing at least one of nickel, palladium, cobalt and gold. From the viewpoint of improving the bonding strength with the first insulating film 12, the first barrier metal 13b is preferably a titanium film, a nickel film, a chromium film, a tungsten film, or a cobalt film. In addition, from the viewpoint of adhesion with the first electrode body 13a and resistance to temperature cycles, the first barrier metal 13b and the second barrier metal 13c are preferably nickel electroplated films or palladium electroplated films. Furthermore, these materials have low ionization tendency and are materials with high barrier performance for preventing the dissolution of materials such as copper constituting the first electrode body 13a. From the viewpoint of barrier performance, the first barrier metal 13b and the second barrier metal 13c are preferably composed of at least one selected from nickel, cobalt and tungsten.

[0059] The second substrate 20 includes a second supporting substrate 21, a second insulating film 22, and a plurality of second electrodes 23. The second insulating film 22 is provided on the second supporting substrate 21. Each second electrode 23 is provided in a second recess 24 formed in the second insulating film 22, and is formed to be exposed from a second surface 22a of the second insulating film 22. The second substrate 20 may have the same structure as the first substrate 10. The second supporting substrate 21 may have the same structure as the first supporting substrate 11. The second insulating film 22 may have the same structure as the first insulating film 12, and the second insulating film 22 is formed of an organic insulating material. The second insulating film 22 may partially contain an inorganic insulating material. Since the structure of the second substrate 20 corresponds to the structure of the first substrate 10, the description of the structures of the second supporting substrate 21 and the second insulating film 22 is omitted.

[0060] The second electrode 23 has the same structure as the first electrode 13, and has a second electrode body 23a, a third barrier metal 23b, and a fourth barrier metal 23c. The second electrode 23 is an electrode corresponding to the first electrode 13, and can be a terminal electrode such as a bump or a wiring electrode as the first electrode 13. The second electrode body 23a is arranged in the second recess 24 formed in the second insulating film 22, and is formed of a material having high conductivity such as copper, aluminum, or silver. The third barrier metal 23b is arranged on the inner surface 24a and the bottom surface 24b of the second recess 24, covering the side surface and the bottom surface of the second electrode body 23a. The thickness of the third barrier metal 23b is, for example, in the range of 0.1μm to 0.8μm. The bonding strength between the second insulating film 22 and the third barrier metal 23b is 30MPa or more. The bonding strength between the second insulating film 22 and the third barrier metal 23b is preferably 40MPa or more, and more preferably 50MPa or more. The fourth barrier metal 23c covers the surface of the second electrode body 23a on the opening side of the second recess 24. The thickness of the fourth barrier metal 23c is, for example, in the range of 0.1 μm to 0.8 μm, and is 1 μm or less before being bonded to the first electrode 13. The second electrode body 23a is entirely covered by the third barrier metal 23b and the fourth barrier metal 23c.

[0061] The third barrier metal 23b and the fourth barrier metal 23c are used to prevent the dissolution into the resin of the second electrode body 23a formed of a material that is easily ionized. They are made of a conductive material with a low ionization tendency, similar to the first barrier metal 13b and the second barrier metal 13c. The third barrier metal 23b and the fourth barrier metal 23c are, for example, composed of at least one selected from titanium, nickel, palladium, chromium, tantalum, tungsten, cobalt and gold. The third barrier metal 23b and the fourth barrier metal 23c are preferably electroplated films (for example, electroless plating films), for example, preferably nickel electroplated films, palladium electroplated films, cobalt electroplated films, gold electroplated films or alloy electroplated films containing at least one of nickel, palladium, cobalt and gold. From the viewpoint of improving the bonding strength with the second insulating film 22, the third barrier metal 23b is preferably a titanium film, a nickel film, a chromium film, a tungsten film, or a cobalt film. Furthermore, from the viewpoint of adhesion to the second electrode body 23a and resistance to temperature cycles, the third barrier metal 23b and the fourth barrier metal 23c are preferably nickel electroplated films or palladium electroplated films. Furthermore, these materials are materials with low ionization tendency and are materials with high barrier performance for preventing the dissolution of materials such as copper constituting the second electrode body 23a. From the viewpoint of barrier performance, the third barrier metal 23b and the fourth barrier metal 23c are preferably composed of at least one selected from nickel, cobalt and tungsten. In the semiconductor device 1, the second barrier metal 13c of the first electrode 13 is bonded to the fourth barrier metal 23c of the second electrode 23.

[0062] (Method for manufacturing semiconductor device)

[0063] Next, refer to Figure 3 to Figure 5 , a method for manufacturing the semiconductor device 1 is described. Figure 3 It is a cross-sectional view for explaining the method of manufacturing the semiconductor device 1 , and shows an example of the process of manufacturing the first substrate 10 and the second substrate 20 . Figure 4 It is a magnified representation Figure 3 (d) is a cross-sectional view of region B shown. Figure 5 is a cross-sectional view for explaining a method of manufacturing the semiconductor device 1. Figure 3 An example of a process of bonding the first substrate 10 and the second substrate 20 is shown.

[0064] The semiconductor device 1 can be manufactured through, for example, the following steps (a) to (d).

[0065] a) A step of preparing a first substrate including a first supporting substrate, a first insulating film provided on the first supporting substrate, and a first electrode provided in a first recessed portion of the first insulating film and exposed from a first surface side of the first insulating film.

[0066] b) a step of preparing a second substrate including a second supporting substrate, a second insulating film provided on the second supporting substrate, and a second electrode provided in a second recessed portion of the second insulating film and exposed from a second surface side of the second insulating film.

[0067] c) A step of bonding the first insulating film of the first substrate and the second insulating film of the second substrate.

[0068] d) A step of bonding the first electrode of the first substrate and the second electrode of the second substrate.

[0069] The above-mentioned step a) of preparing the first substrate includes the following steps.

[0070] a1) Step of forming a first insulating film on a first supporting substrate

[0071] a2) Step of forming at least one first recessed portion in the first insulating film

[0072] a3) Step of forming a first barrier metal on the inner surface and bottom surface of the first recess

[0073] a4) forming a first electrode body in the first recess and in a region surrounded by the first barrier metal

[0074] a5) Step of forming a second barrier metal on the surface of the first electrode body

[0075] Furthermore, the step b) of preparing the second substrate includes the following steps.

[0076] b1) Step of forming a second insulating film on a second supporting substrate

[0077] b2) Step of forming at least one second recess in the second insulating film

[0078] b3) Step of forming a third barrier metal on the inner surface and bottom surface of the second recess

[0079] b4) forming a second electrode body in the second recess and in a region surrounded by the third barrier metal

[0080] b5) Step of forming a fourth barrier metal on the surface of the second electrode body

[0081] [Step (a)]

[0082] The method of manufacturing (preparing) the first substrate 10 is described. To manufacture the first substrate 10, first prepare the first support substrate 11. The first support substrate 11 is, for example, a substrate with a thickness of 0.2 mm to 2.0 mm and a wafer-shaped or panel-shaped substrate. The first support substrate 11 may have other configurations. Figure 3As shown in (a), the first insulating film 12 is formed on the first supporting substrate 11. For example, when the first insulating film 12 is formed of a photosensitive insulating film, the first insulating film 12 is formed by laminating the photosensitive insulating film on the first supporting substrate 11. As for the material of the insulating film, the insulating film described above can be used. The lamination temperature can be, for example, 40°C to 120°C. The photosensitive insulating film used therein can be an insulating film containing a thermosetting organic insulating material. In addition, the method for forming the first insulating film 12 is not limited thereto, and can be formed by other methods. For example, when the first insulating film 12 is formed of a liquid organic insulating material, the first insulating film 12 can be formed by applying the insulating material on the first supporting substrate 11 and then rotating the first supporting substrate 11. The thickness of the first insulating film 12 formed on the first supporting substrate 11 is, for example, preferably less than 10 μm, less than 5 μm, and more preferably less than 3 μm. In addition, the thickness of the first insulating film 12 can be greater than 1 μm. Alternatively, the first insulating film 12 may be formed of an inorganic material.

[0083] Next, according to Figure 3 As shown in (b), a plurality of first recesses 14 are formed in the first insulating film 12. The first recesses 14 can be formed, for example, by laser ablation, photolithography, imprinting, etc. In the case of using a photolithography process, a fine first recess 14 can be produced at a low cost. In the case of forming the recesses by using a photolithography process, it is preferred to use a film-shaped photosensitive organic insulating material in the first insulating film 12. As an exposure method for the photosensitive organic insulating material, a conventional projection exposure method, a contact exposure method, a direct drawing exposure method, etc. can be used. As a developing method, a method of developing with an alkaline aqueous solution of sodium carbonate or TMAH can be used. After the first recess 14 is formed, the insulating material (thermosetting material) constituting the first insulating film 12 can be further heated and cured. The heating temperature at this time is, for example, 100°C to 200°C, and the heating time can be, for example, between 30 minutes and 3 hours. The first recess 14 formed by the above method has an opening diameter or opening width of 5 μm or more and 50 μm or less.

[0084] Next, when the first insulating film 12 forms a plurality of first recesses 14, the first barrier metal 13b is formed on the inner surface 14a and the bottom surface 14b of the first recess 14. In the step of forming the first barrier metal 13b, Figure 3As shown in (b), on the inner surface 14a and the bottom surface 14b of the first recess 14 and the first surface 12a of the first insulating film 12, a conductive material 3A constituting the first barrier metal 13b is formed by electroplating (electroless plating) or the like. At this time, the first barrier metal is formed in such a way that the bonding strength between the first insulating film 12 and the first barrier metal 13b becomes 30 MPa or more. The bonding strength between the first insulating film 12 and the first barrier metal 13b may be 40 MPa or more, or 50 MPa or more. The conductive material 3A forming the first barrier metal 13b includes, for example, at least one selected from titanium, nickel, palladium, chromium, tantalum, tungsten, cobalt and gold. Since the first barrier metal 13b also acts as a seed layer for forming the first electrode body 13a described later, it may be any one of titanium, copper, nickel, nickel alloy (NiP, NiB, CoNiP), cobalt, and tungsten alloy (Taw). These materials are applied by, for example, electroless plating.

[0085] Among them, the bonding strength when the barrier film is given to the organic material film is described. In the case where copper is directly set on the organic material film without inserting a barrier film, the copper oxidizes over time and peels off from the organic material film. However, in the case where a barrier film is inserted on the organic material film and a copper electrode is set, such peeling is prevented. For example, the inventors used a photosensitive insulating material (manufactured by Resonac Corporation, product name AH-3000) as an organic material film, and a NiB film (manufactured by JCU CORPORATION, product name) as a barrier film, and formed a barrier film on the organic material film by electroless nickel boron plating. The thickness of the barrier film formed is 100nm. The formation conditions of the barrier film are electroless plating. The test piece was subjected to a peel strength test of the barrier film and the organic material film. The peel strength at this time is, for example, 40MPa. That is, it was confirmed by the above method that the bonding strength between the first insulating film 12 and the first barrier metal 13b can be set to 30MPa or more or 40MPa or more. In addition, by changing the type of organic insulating film or barrier film used, the bonding strength between the first insulating film 12 and the first barrier metal 13b can be further set to 50 MPa or more. The above insulating film can also be applied to the bonding strength between the second insulating film 22 and the third barrier metal 23b described later.

[0086] Next, when the first barrier metal 13b (conductive material 3A) is formed, the first electrode body 13a is formed in the first recess 14 and in the region surrounded by the first barrier metal 13b. In the step of forming the first electrode body 13a, Figure 3As shown in (c), on the conductive material 3A formed in the first recess 14 and on the first insulating film 12, a conductive material 3B constituting the first electrode body 13a is formed by electroplating or the like. The conductive material 3B forming the first electrode body 13a includes, for example, at least one selected from copper, aluminum, and silver. The first electrode body 13a (conductive material 3B) is electroplated to form a first barrier metal 13b (conductive material 3A) that acts as a seed layer as a power supply layer. When forming the first electrode body 13a, a conductive material, such as copper, is precipitated on the first barrier metal 13b in the first recess 14 and on the first insulating film 12 to bury the first recess 14.

[0087] Next, when the conductive material 3B for forming the first electrode body 13a is formed, the conductive material 3A of the first barrier metal 13b and the conductive material 3B of the first electrode body 13a are ground to remove unnecessary portions, thereby forming the first barrier metal 13b and the first electrode body 13a of a specific thickness. In addition, when this grinding is performed, the first insulating film 12 can be ground together with the conductive material 3A and the conductive material 3B to set the thickness to a specific value.

[0088] Next, when the first electrode body 13a and the first barrier metal 13b are formed, the first surface 12a of the first insulating film 12 is polished. This polishing can be performed using a grinder for electronic material processing or a method based on CMP (Chemical Mechanical Polishing). The surface roughness of the first surface 12a of the first insulating film 12 is reduced to 0.1 μm or less by this polishing. The surface roughness used here is the arithmetic mean roughness Ra measured at a magnification of 20 times using a laser microscope, and is the arithmetic mean roughness Ra specified by JIS B 0601 2001. When performing this polishing, the surface of the first electrode body 13a can be polished under the condition that the surface of the first insulating film 12 is coplanar, the surface of the first electrode body 13a protrudes more than the first surface 12a of the first insulating film 12, or the surface of the first electrode body 13a is recessed inwardly from the first surface 12a of the first insulating film 12. As an example, the first insulating film 12 is polished so that the surface of the first electrode body 13a is slightly recessed inward from the first surface 12a of the first insulating film 12. Such conditions can be controlled by appropriately adjusting the polishing liquid and polishing conditions used for CMP.

[0089] Next, when the surfaces of the first insulating film 12 and the first electrode body 13a are polished, the surface of the first electrode body 13a is modified by at least one of ultraviolet irradiation, electron beam irradiation, ozone water treatment, corona discharge treatment, and plasma treatment. This surface modification is a treatment before forming the second barrier metal 13c described later.

[0090] Next, according to Figure 3 As shown in (d), a second barrier metal 13c is formed on the surface of the first electrode body 13a. In this process, after the above-mentioned process of grinding the conductive material and pre-treating the surface of the first electrode body, the second barrier metal is formed in a manner covering the surface of the first electrode body 13a. The second barrier metal 13c is formed on the first electrode body 13a, for example, by electroless plating. The second barrier metal 13c is formed, for example, of at least one material selected from titanium, nickel, palladium, chromium, tantalum, tungsten, cobalt and gold. The second barrier metal 13c is formed of a material with a small ionization tendency. In addition, when the second barrier metal 13c is formed by electroless plating, the material can be formed in a manner covering the first surface 12a of the first insulating film 12 according to the formation of the first barrier metal 13b, but at this time, the excess material is ground or polished in the same manner as described above. The first substrate 10 is prepared by the above process.

[0091] [Step (b)]

[0092] Since the manufacturing method of the second substrate 20 is the same as the manufacturing method of the first substrate 10, the detailed description is omitted. Figure 3 The second substrate 20 is manufactured by the process shown in Figure 3 and Figure 5 In the example shown in , the second substrate 20 has the same structure as the first substrate 10, but it does not need to be exactly the same as the first substrate 10. The thickness or forming material of the second supporting substrate 21, the thickness or forming material of the second insulating film 22, the presence or absence of a semiconductor chip, etc. can be different from the first substrate 10.

[0093] [Step (c)]

[0094] Next, when the preparation of the first substrate 10 and the second substrate 20 is completed, the first insulating film 12 of the first substrate 10 and the second insulating film 22 of the second substrate 20 are bonded together. Figure 5As shown in (a), at least one of the first substrate 10 and the second substrate 20 is aligned in such a manner that the first electrode 13 of the first substrate 10 and the second electrode 23 of the second substrate 20 correspond to each other. Both the first substrate 10 and the second substrate 20 may be aligned. For such alignment, an alignment mark or the like may be provided on at least one of the first substrate 10 and the second substrate 20.

[0095] In step (c), after removing the organic matter or metal oxide attached to the surfaces of the first substrate 10 and the second substrate 20, the first substrate 10 and the second substrate 20 are aligned. When the alignment is completed, the first insulating film 12 of the first substrate 10 and the second insulating film 22 of the second substrate 20 are bonded to each other as a hybrid bond. At this time, the bonding can be performed after the first insulating film 12 of the first substrate 10 and the second insulating film 22 of the second substrate 20 are uniformly heated. The temperature difference between the first substrate 10 and the second substrate 20 during bonding is preferably 10° C. or less, for example. By such heat bonding at a uniform temperature, the first insulating film 12 is mechanically and firmly attached to the second insulating film 22. In addition, since the heat bonding is performed at a uniform temperature, it is difficult to cause positional deviation at the bonding point, and high-precision bonding can be performed. In the bonding stage, the first electrode 13 of the first substrate 10 and the second electrode 23 of the second substrate 20 are spaced apart from each other and are not bonded (but aligned). In addition, the first substrate 10 and the second substrate 20 may be bonded together by other bonding methods, for example, bonding by room temperature bonding or the like.

[0096] [Step (d)]

[0097] Next, when the bonding of the first substrate 10 and the second substrate 20 is completed, the plurality of first electrodes 13 of the first substrate 10 and the plurality of second electrodes 23 of the second substrate 20 are bonded to each other. Figure 5 As shown in (b), when the bonding of step (c) is completed, a specific heat or pressure or both are applied to bond the first electrode 13 of the first substrate 10 and the second electrode 23 of the second substrate 20 as a mixed bonding. When the first electrode 13 and the second electrode 23 are composed of copper, for example, the annealing temperature in step (d) is preferably 150°C or more and 400°C or less, and more preferably 200°C or more and 300°C or less. The electrode bonding portion where the first electrode 13 and the corresponding second electrode 23 are bonded by this bonding treatment is mechanically and electrically firmly bonded to the first electrode 13 and the second electrode 23. In addition, the electrode bonding of step (d) can be performed after the bonding of step (c), but can also be performed at the same time as the bonding of step (c).

[0098] Made through the above process Figure 1The semiconductor device 1 is shown in FIG.

[0099] Among them, reference Figure 6 and Figure 7 , the method for manufacturing a semiconductor device according to the present embodiment is compared with the method for manufacturing a semiconductor device in a comparative example, and the effects of the method for manufacturing a semiconductor device according to the present embodiment are described. Figure 6 This is a cross-sectional view showing an example in which positional deviation occurs when the first substrate 10 and the second substrate 20 are bonded together and the first electrode 13 and the second electrode 23 are joined. Figure 7 (a) is a cross-sectional view showing a case where positional deviation occurs at a junction of a semiconductor device 1A manufactured by the method of this embodiment. Figure 7 (b) is a cross-sectional view showing a semiconductor device manufactured by the method of the comparative example when positional displacement occurs at the junction. In the manufacturing method of the comparative example, the first electrode 113 corresponding to the first electrode 13 and the second electrode 123 corresponding to the second electrode 23 are not provided with metal caps corresponding to the second barrier metal 13c and the fourth barrier metal 23c, which is different from the manufacturing method of the embodiment. The other steps and structures are the same as those of the embodiment.

[0100] In the case of such positional deviation, according to Figure 7 As shown in (b), in the manufacturing method of the semiconductor device of the comparative example, the positional deviation S causes the first electrode body 113a of the first electrode 113 to be exposed to the resin side constituting the second insulating layer 121. Similarly, the second electrode body 123a of the second electrode 123 is exposed to the resin side constituting the first insulating layer 111. At this time, copper and the like constituting the first electrode body 113a and the second electrode body 123a are dissolved, resulting in migration between the electrode and the resin. As a result, for example, a short circuit occurs between the terminal electrodes.

[0101] In contrast, in the manufacturing method of the semiconductor device 1, 1A and the semiconductor device 1, 1A of the present embodiment, the surface of the first electrode body 13a of the first electrode 13 is covered by the second barrier metal 13c, and the entire first electrode body 13a is covered by the first barrier metal 13b and the second barrier metal 13c. Similarly, the surface of the second electrode body 23a of the second electrode 23 is covered by the fourth barrier metal 23c, and the entire second electrode body 23a is covered by the third barrier metal 23b and the fourth barrier metal 23c. At this time, the dissolution of the first electrode body 13a and the second electrode body 23a, which are mostly formed of a material that is easily dissolved, such as copper, is suppressed by the first barrier metal 13b and the second barrier metal 13c and the third barrier metal 23b and the fourth barrier metal 23c. Thus, even if positional deviation occurs between the first electrode 13 and the second electrode 23 at any stage, migration of the interface between the first electrode 13 and the first insulating film 12 can be suppressed, and migration of the interface between the second electrode 23 and the second insulating film 22 can be suppressed.

[0102] In addition, sometimes the electrode material such as copper is weakly bonded to the resin constituting the insulating film, which sometimes causes peeling. However, in the manufacturing method of the semiconductor device 1, 1A of the present embodiment, such peeling can be suppressed by providing the first barrier metal 13b on the inner surface 14a and the bottom surface 14b of the first recess 14 of the first insulating film 12 and covering a part of the first electrode body 13a, and the bonding strength between the first insulating film 12 and the first barrier metal 13b is 30 MPa or more. Similarly, such peeling can be suppressed by providing the third barrier metal 23b on the inner surface 24a and the bottom surface 24b of the second recess 24 of the second insulating film 22 and covering a part of the second electrode body 23a, and the bonding strength between the second insulating film 22 and the third barrier metal 23b is 30 MPa or more.

[0103] Furthermore, in the manufacturing method of the semiconductor device 1, 1A of the present embodiment, the first insulating film 12 and the second insulating film 22 include organic insulating films. At this time, foreign matter (fragments) attached to the surface of the first substrate 10 and the second substrate 20 can be absorbed into the insulating film by a relatively soft material, namely an organic material, so as to reduce the poor connection between the first substrate 10 and the second substrate 20. The organic insulating material contained in the insulating film can be polyimide, a polyimide precursor, polyamide-imide, benzocyclobutene (BCB), polybenzoxazole (PBO) or a PBO precursor. Since these materials are soluble in liquid or solvent, it is easy to make an insulating film by, for example, spin coating, and it is easy to form a thin film. Furthermore, since these materials have high heat resistance, they can withstand the high temperature when joining the first substrate 10 and the second substrate 20, and the first substrate 10 and the second substrate 20 can be joined more reliably.

[0104] Furthermore, in the method for manufacturing the semiconductor device 1, 1A of the present embodiment, the thickness of the second barrier metal 13c and the fourth barrier metal 23c before joining the first electrode 13 and the second electrode 23 can be 1 μm or less. In this case, the terminal electrode can be miniaturized more reliably.

[0105] Furthermore, in the method for manufacturing the semiconductor device 1, 1A of the present embodiment, when the first electrode 13 and the second electrode 23 are bonded, the second barrier metal 13c and the fourth barrier metal 23c are bonded. Thus, even if positional displacement occurs between the first electrode 13 and the second electrode 23, a portion of at least one of the second barrier metal 13c and the fourth barrier metal 23c is bonded to the resin to prevent the first electrode body 13a and the second electrode body 23a from being bonded to the resin. Thus, migration of the interface between the first electrode 13 and the first insulating film 12 and the interface between the second electrode 23 and the second insulating film 22 can be more reliably suppressed.

[0106] Furthermore, in the method for manufacturing the semiconductor device 1, 1A of the present embodiment, the second barrier metal 13c and the fourth barrier metal 23c may be formed to include at least one selected from titanium, nickel, palladium, chromium, tantalum, tungsten, cobalt, and gold. Since the second barrier metal 13c and the fourth barrier metal 23c include such a material with high barrier capability, migration at the interface between the first electrode 13 and the first insulating film 12 and at the interface between the second electrode 23 and the second insulating film 22 can be more reliably suppressed.

[0107] In addition, in the above-mentioned manufacturing method, although the case where the first insulating film 12 and the second insulating film 22 include an organic insulating film is described, it is not limited to this. In the manufacturing method of the semiconductor device of this embodiment, the first insulating film 12 and the second insulating film 22 may further include an inorganic insulating film. When the insulating film includes an inorganic insulating film, it is easy to miniaturize the recessed portion for the terminal electrode, etc., so it is possible to manufacture a semiconductor device 1, 1A with finer wiring. In addition, since it is easy to firmly bond inorganic materials to each other, it is possible to improve the connection reliability as a semiconductor device by improving the bonding strength between the first substrate 10 and the second substrate 20.

[0108] Furthermore, in the method for manufacturing the semiconductor device 1, 1A of the present embodiment, the first insulating film 12 and the second insulating film 22 can be polished by CMP or the like, and the surface roughness of the polished first insulating film 12 and the second insulating film 22 can be 0.1 μm or less. Thus, the bonding strength when the first insulating film 12 and the second insulating film 22 are bonded can be improved.

[0109] In the manufacturing method of the semiconductor device 1, 1A of the present embodiment, before the process of forming the second barrier metal 13c, the surface of the first electrode body 13a can be surface-modified by at least one of ultraviolet irradiation, electron beam irradiation, ozone water treatment, corona discharge treatment, and plasma treatment. As a result, the bonding strength of the second barrier metal 13c to the first electrode body 13a can be improved, and migration can be suppressed by suppressing the peeling of the second barrier metal 13c. And, similarly, before the process of forming the fourth barrier metal 23c, the surface of the second electrode body 23a can be surface-modified by at least one of ultraviolet irradiation, electron beam irradiation, ozone water treatment, corona discharge treatment, and plasma treatment. As a result, the bonding strength of the fourth barrier metal 23c to the second electrode body 23a can be improved, and migration can be suppressed by suppressing the peeling of the fourth barrier metal 23c.

[0110] [First Modification]

[0111] Among them, reference Figure 8 , a first variation of the method for manufacturing a semiconductor device according to the present embodiment is described. Figure 8 1 is a cross-sectional view for explaining a first variation of the method for manufacturing a semiconductor device according to the present embodiment. Figure 8 As shown in (a), in the method for manufacturing a semiconductor device of the first modified example, in step (a), the first electrode 13A is formed in such a manner that the surface of the second barrier metal 13c is recessed inwardly relative to the first surface 12a of the first insulating film 12. In order to form such a recessed area 13d, it is possible to achieve this by controlling at least one of the depth of the first recess 14, the thickness of the first barrier metal 13b, the amount of the conductive material constituting the first electrode body 13a or the position of the surface of the first electrode body 13a, the grinding or polishing conditions of the first insulating film 12 and the first electrode body 13a, the thickness or amount of the disposed second barrier metal 13c, and the like.

[0112] Furthermore, in the method for manufacturing a semiconductor device according to the first modification, in step (b), the second electrode 23A is formed in such a manner that the surface of the fourth barrier metal 23c protrudes outward from the second surface 22a of the second insulating film 22. In order to form such a protruding portion 23d, it is possible to control at least one of the depth of the second recess 24, the thickness of the third barrier metal 23b, the amount of the conductive material constituting the second electrode body 23a or the position of the surface of the second electrode body 23a, the grinding or polishing conditions of the second insulating film 22 and the second electrode body 23a, the thickness or amount of the disposed fourth barrier metal 23c, and the like.

[0113] Next, in the manufacturing method of the first variant, according to Figure 8As shown in (b), when the first insulating film 12 and the second insulating film 22 are bonded together in step (c), the protruding portion 23d of the fourth barrier metal 23c is embedded in the recessed area 13d of the second barrier metal 13c. By this concave-convex structure, in the manufacturing method of the first variant, the first substrate 10 and the second substrate 20 are more accurately aligned to prevent positional deviation. Thereafter, in step (d), the first electrode 13A is bonded to the second electrode 23A. In the manufacturing method of the semiconductor device of the first variant, in addition to the effect of preventing the dissolution of copper such as the second barrier metal 13c and the fourth barrier metal 23c, positional deviation during bonding can be prevented by having this alignment structure. As a result, migration of the interface between the electrode and the insulating film can be further suppressed.

[0114] [Second Modification]

[0115] Next, refer to Fig. 9 A second modified example of the method for manufacturing a semiconductor device according to the present embodiment will be described. Fig. 9 2 is a cross-sectional view for explaining a second variation of the method for manufacturing a semiconductor device according to the present embodiment. In the above embodiment, an example in which the first electrode 13 and the second electrode 23 have the same width is used for explanation, but the present invention is not limited to this. Fig. 9 As shown, the width of the first electrode 13B may be formed to be wider than the width of the second electrode 23. In this case, even if the second electrode 23 is slightly offset relative to the first electrode 13B, the entire second electrode 23 can be bonded to the first electrode 13B. The width of the first electrode 13B may be, for example, greater than 1.0 times and less than 3.0 times the width of the second electrode 23. In this case, even if a slight positional offset occurs, migration of the interface between the electrode and the insulating film can be suppressed.

[0116] [Third Modification]

[0117] Next, refer to Fig.10 , a third variation of the method for manufacturing a semiconductor device according to the present embodiment is described. Fig.10 FIG. 1 is a cross-sectional view for explaining a third variant of the method for manufacturing a semiconductor device according to the present embodiment. In the third variant, similarly to the second variant, Fig.10As shown, the width of the first electrode 13B is formed to be wider than the width of the second electrode 23C. On the other hand, in this modification, the first electrode 13B has the second barrier metal 13c, but the second electrode 23C does not have the fourth barrier metal 23c. At this time, even if the second electrode 23C is slightly offset relative to the first electrode 13B, since the entire second electrode 23C can be bonded to the first electrode 13B, even if there is a slight positional offset, migration of the interface between the electrode and the insulating film can be suppressed. By providing a metal cap, i.e., a barrier metal, on at least one of them in this way, migration can be suppressed.

[0118] Although the embodiment of the present invention has been described above, the present invention is not limited to the above-described embodiment, and can be appropriately modified within a scope not departing from the gist of the present invention.

[0119] Explanation of symbols

[0120] 1, 1A-semiconductor device, 10-first substrate, 11-first supporting substrate, 12-first insulating film, 12a-first surface, 13, 13A, 13B-first electrode, 13a-first electrode body, 13b-first barrier metal, 13c-second barrier metal, 13d-recessed area, 14-first recessed portion, 14a-inner surface, 14b-bottom surface, 20-second substrate, 21-second supporting substrate, 22-second insulating film, 22a-second surface, 23, 23A, 23C-second electrode, 23a-second electrode body, 23b-third barrier metal 23c-fourth barrier metal, 23d-protruding portion, 30, 40-semiconductor chip (semiconductor element).

Claims

1. A method for manufacturing a semiconductor device, comprising: a step of preparing a first substrate, the first substrate having a first supporting substrate, a first insulating film provided on the first supporting substrate, and a first electrode provided in a first recessed portion of the first insulating film and exposed from a first surface side of the first insulating film; a step of preparing a second substrate, the second substrate having a second supporting substrate, a second insulating film provided on the second supporting substrate, and a second electrode provided in a second recessed portion of the second insulating film and exposed from a second surface side of the second insulating film; a step of bonding the first insulating film of the first substrate and the second insulating film of the second substrate; and a step of bonding the first electrode of the first substrate and the second electrode of the second substrate, The first insulating film includes an organic insulating film, and the first electrode includes: a first electrode body disposed in the first concave portion; a first barrier metal disposed on at least one of an inner surface and a bottom surface of the first concave portion and covering a portion of the first electrode body; and a second barrier metal covering the surface of the first electrode body on the opening side of the first recess, wherein the bonding strength between the first insulating film and the first barrier metal is 30 MPa or more.

2. The method for manufacturing a semiconductor device according to claim 1, wherein: The bonding strength between the first insulating film and the first barrier metal is 40 MPa or more.

3. The method for manufacturing a semiconductor device according to claim 1 or 2, wherein: The step of preparing the first substrate includes: forming the first insulating film on the first supporting substrate; forming at least one first recess in the first insulating film; forming the first barrier metal on the inner surface and the bottom surface of the first recess; forming the first electrode body in the first recess and in a region surrounded by the first barrier metal; and The step of forming a second barrier metal on the surface of the first electrode body.

4. The method for manufacturing a semiconductor device according to claim 3, wherein: In the step of forming the first barrier metal, the first barrier metal is formed in the first recessed portion of the first insulating film by electroless plating.

5. The method for manufacturing a semiconductor device according to claim 4, wherein: In the step of forming the first electrode body, the first electrode body is formed by electroplating using the first barrier metal as a power supply layer.

6. The method for manufacturing a semiconductor device according to any one of claims 3 to 5, wherein: In the step of forming the first electrode body, a conductive material is disposed on the first barrier metal and the first insulating film in the first recess so as to at least fill the first recess, and the disposed conductive material is ground to form the first electrode body.

7. The method for manufacturing a semiconductor device according to claim 6, wherein: In the step of forming the first electrode body, the first insulating film is polished after the conductive material is ground, and the surface roughness of the first insulating film after the polishing is 0.1 μm or less.

8. The method for manufacturing a semiconductor device according to claim 6 or 7, wherein: In the step of forming the second barrier metal, after grinding the conductive material, the second barrier metal is formed so as to cover the surface of the first electrode body.

9. The method for manufacturing a semiconductor device according to any one of claims 3 to 8, wherein: The step of preparing the first substrate includes: before the step of forming the second barrier metal, the step of modifying the surface of the first electrode body by at least any one of ultraviolet irradiation, electron beam irradiation, ozone water treatment, corona discharge treatment and plasma treatment.

10. The method for manufacturing a semiconductor device according to any one of claims 1 to 9, wherein: The entire first electrode body is covered by the first barrier metal and the second barrier metal.

11. The method for manufacturing a semiconductor device according to any one of claims 1 to 10, wherein: The thickness of the second barrier metal before the first electrode and the second electrode are bonded is 1 μm or less.

12. The method for manufacturing a semiconductor device according to any one of claims 1 to 11, wherein: The second insulating film includes an organic insulating film, and the second electrode includes: a second electrode body, which is arranged in the second recess; a third barrier metal, which is arranged on at least one of the inner surface and the bottom surface of the second recess and covers a portion of the second electrode body; and a fourth barrier metal, which covers the surface of the second electrode body on the opening side of the second recess, and the bonding strength between the second insulating film and the third barrier metal is greater than 30 MPa.

13. The method for manufacturing a semiconductor device according to claim 12, wherein: The first electrode is formed in such a manner that a surface of the second barrier metal is recessed inwardly from the first surface of the first insulating film. The second electrode is formed in such a manner that a surface of the fourth barrier metal protrudes outward from the second surface of the second insulating film. In the step of bonding the first insulating film and the second insulating film, the protruding portion of the fourth barrier metal is embedded in the recessed region of the second barrier metal.

14. The method for manufacturing a semiconductor device according to any one of claims 1 to 13, wherein: At least one semiconductor element is arranged in the first supporting substrate or on a surface of the first supporting substrate opposite to a surface on which the first insulating film is formed.

15. A semiconductor device comprising: a first substrate including a first supporting substrate, a first insulating film provided on the first supporting substrate, and a first electrode provided in a first recessed portion of the first insulating film and exposed from a first surface side of the first insulating film; and The second substrate includes a second supporting substrate, a second insulating film provided on the second supporting substrate, and a second electrode provided in a second recessed portion of the second insulating film and exposed from a second surface side of the second insulating film. The first insulating film includes an organic insulating film, The first insulating film is bonded to the second insulating film. The first electrode is joined to the second electrode, The first electrode comprises: a first electrode body, arranged in the first recess; a first barrier metal, arranged on at least one of the inner surface and the bottom surface of the first recess and covering a portion of the first electrode body; and a second barrier metal, covering the surface of the first electrode body on the opening side of the first recess, and the bonding strength between the first insulating film and the first barrier metal is greater than 30 MPa.

16. The semiconductor device according to claim 15, wherein: The second insulating film includes an organic insulating film, The second electrode comprises: a second electrode body, which is arranged in the second recess; a third barrier metal, which is arranged on at least one of the inner surface and the bottom surface of the second recess and covers a portion of the second electrode body; and a fourth barrier metal, which covers the surface of the second electrode body on the opening side of the second recess, and the bonding strength between the second insulating film and the third barrier metal is greater than 30 MPa.