Preparation method of efficient silica gel monolithic column for refining 2-amino-5-bromopyridine
By using aqueous ammonia solution in a silica gel column to optimize the pore structure and the modification treatment of amino-modified graphene oxide materials, the problems of low separation efficiency and hygroscopicity of 2-amino-5-bromopyridine are solved, and efficient refining and stable products are achieved Output.
Patent Information
- Application Number
- CN202411305147.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-29
AI Technical Summary
The existing 2-amino-5-bromopyridine is poor in separation efficiency during the purification process, easily introduces impurities, difficult crystallization and high hygroscopicity lead to deterioration of the product. The traditional silica gel column cannot be effectively separated without modification.
The double-pore structure of the silica gel column is optimized by using aqueous ammonia solution as the pore-making agent, and the modification of amino-modified graphene oxide material is improved to improve the chromatographic separation performance of the silica gel column and reduce deformation and cracking caused by drying.
It improves the refining efficiency of 2-amino-5-bromopyridine, enhances the separation performance of the overall column of silica gel, reduces the influence of impurities introduction and hygroscopicity, and ensures the purity and stability of the product.
Smart Images

Figure BDA0005048925470000071 
Figure BDA0005048925470000081
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a high-efficiency silica gel monolithic column for refining 2-amino-5-bromopyridine, and belongs to the technical field of refining 2-amino-5-bromopyridine. Background Art
[0002] 2-Amino-5-bromopyridine is a chemical substance with the molecular formula C5H5BrN2. It is a white crystalline solid powder and belongs to the pyridine derivatives. It has significant alkalinity and the common chemical properties of pyridine. It can be used as an intermediate in organic synthesis and pharmaceutical chemistry, and is mostly used in basic chemical research and the preparation process of drug molecules.
[0003] Existing 2-amino-5-bromopyridine is in the process of generation, because 2-amino-5-bromopyridine is in the process of synthesis, some impurities may be introduced, such as unreacted raw materials, catalysts, by-products, etc. These impurities can affect the purity and quality of the product, and need to be effectively removed. And the crystallization separation process of 2-amino-5-bromopyridine may be difficult, and caking or uneven situations may occur easily, affecting the quality and output of the product. Meanwhile, because 2-amino-5-bromopyridine has higher hygroscopicity, it is easy to absorb moisture in the air, causing the product to deteriorate or affecting its performance.
[0004] In view of the above-mentioned related technologies, the inventors found that in the existing refining process of 2-amino-5-bromopyridine, a chromatographic separation scheme is often used to treat it, but the traditional silica gel monolithic column has not been modified, and its separation effect is poor, and 2-amino-5-bromopyridine cannot be separated and purified efficiently. Summary of the invention
[0005] In order to improve the problem of poor separation efficiency of the existing silica gel monolithic column for purifying 2-amino-5-bromopyridine, the present application provides a method for preparing a high-efficiency silica gel monolithic column for purifying 2-amino-5-bromopyridine.
[0006] A method for preparing a high-efficiency silica gel monolithic column for refining 2-amino-5-bromopyridine comprises the following preparation steps:
[0007] Take polyethylene glycol, acetic acid and water, stir and mix, and collect the mixed solution;
[0008] After adding tetramethoxysilane to the mixed solution, stirring at low temperature and placing in a water bath, stirring and aging in a water bath environment, collecting a wet silica gel column, taking the wet silica gel column and treating it with 1.5 mol / L ammonia water to collect a silica gel column;
[0009] The silica gel column is immersed in washing treatment, dried and then calcined, left to cool and immersed in a hydrochloric acid solution, and washed with water until neutral, so as to prepare the high-efficiency silica gel monolithic column for purifying 2-amino-5-bromopyridine.
[0010] Through the above technical scheme, the present application optimizes the preparation process of the silica gel monolithic column. The present application adopts an ammonia solution as a pore-forming agent. By optimizing the solubility of ammonia solution, the silica gel monolithic column prepared in the present application has an excellent double pore structure of macropores and mesopores, thereby improving the defect of poor separation efficiency of a single pore size, thereby effectively improving the refining efficiency of 2-amino-5-bromopyridine.
[0011] Furthermore, the immersion solutions used in the immersion washing treatment are nitric acid solution, water and N,N-dimethylformamide in sequence.
[0012] Through the above technical scheme, the present application optimizes the preparation process of the silica gel monolithic column. Since the traditional silica gel monolithic column needs to be dried during the preparation process, the drying process will cause the gel to deform or crack. The present application selects N, N-dimethylformamide as the modified material, first volatilizes the substances with high volatility and high surface tension during the drying process, and then slowly volatilizes N, N-dimethylformamide to reduce the drying rate, thereby reducing the cracking phenomenon.
[0013] Furthermore, the addition ratio of the polyethylene glycol, acetic acid and water is (7-10):1:(100-120).
[0014] Through the above technical scheme, the present application optimizes the material ratio for preparing the silica gel monolithic column of the present application, and the optimized raw materials have good structural performance and chromatographic separation performance.
[0015] Furthermore, it also includes extraction enrichment modification treatment, and the extraction enrichment modification treatment includes the following steps:
[0016] The modified dispersion was subjected to ultrasonic dispersion treatment and then injected into a high-efficiency silica gel monolithic column for 2-amino-5-bromopyridine purification at 30 μL / min. After end-capping, the column was placed at 38-45°C for heat preservation and reaction. After the column was cooled to room temperature, it was rinsed with deionized water and methanol in turn and dried to complete the extraction, enrichment and modification treatment.
[0017] Furthermore, the modified dispersion is amino-modified graphene oxide.
[0018] Through the above technical scheme, the present application modifies the silica gel monolith by using the amino-modified graphene oxide material as the main modification material. Since the graphene oxide material is a material with a two-dimensional spatial structure and contains rich functional groups such as hydroxyl and carboxyl groups, it can effectively modify and modify the silica gel monolith. At the same time, in the amino-modified graphene oxide material, the amino-modified material can react with the carboxyl group on the graphene surface to improve the roughness and specific surface area of the graphene oxide material, thereby further improving the enrichment performance of the silica gel monolithic column material and the chromatographic separation performance of 2-amino-5-bromopyridine.
[0019] Furthermore, the modified dispersion is prepared by the following scheme:
[0020] Graphene oxide and deionized water are stirred and mixed, and a dispersion is collected by ultrasonic dispersion;
[0021] The modified dispersion is prepared by mixing the dispersion and diaminoguanidine hydrochloride, adding glutaraldehyde, adjusting the pH to 10.0, treating the mixture in a water bath, and performing ultrasonic dispersion.
[0022] Through the above technical scheme, the present application selects diaminoguanidine hydrochloride as the amino-modified material, through which it can be effectively loaded onto the surface of graphene oxide. Through the amidation reaction, the specific surface area of the graphene oxide material is further increased, thereby improving the chromatographic separation efficiency of the silica gel monolithic column.
[0023] Furthermore, the water bath treatment temperature is 30-40°C.
[0024] In summary, this application has the following beneficial effects:
[0025] First, the present application optimizes the preparation process of the silica gel monolithic column. The present application adopts an ammonia solution as a pore-forming agent and optimizes the solubility of ammonia solution so that the silica gel monolithic column prepared in the present application has an excellent dual-pore structure of macropores and mesopores, thereby improving the defect of poor separation efficiency of a single pore size, thereby effectively improving the refining efficiency of 2-amino-5-bromopyridine.
[0026] Second, the present application optimizes the preparation process of the silica gel monolithic column. Since the traditional silica gel monolithic column needs to be dried during the preparation process, the drying process will cause the gel to deform or crack. The present application selects N, N-dimethylformamide as the modified material. The substances with high volatility and high surface tension are first volatilized during the drying process, and then the N, N-dimethylformamide is slowly volatilized to reduce the drying rate, thereby reducing the cracking phenomenon.
[0027] Third, the present application uses amino-modified graphene oxide material as the main modification material to modify the silica gel monolithic column. Since the graphene oxide material is a material with a two-dimensional spatial structure and contains rich functional groups such as hydroxyl and carboxyl groups, it can effectively modify and modify the silica gel monolithic column. At the same time, in the amino-modified graphene oxide material, the amino-modified material can react with the carboxyl group on the graphene surface to improve the roughness and specific surface area of the graphene oxide material, thereby further improving the enrichment performance of the silica gel monolithic column material and the chromatographic separation performance of 2-amino-5-bromopyridine. DETAILED DESCRIPTION
[0028] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the invention.
[0029] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.
[0030] There is no particular limitation on the purity of all raw materials in the present invention. The present invention preferably adopts analytical purity or conventional purity requirements in the preparation field.
[0031] The brands and abbreviations of all raw materials of the present invention are conventional brands and abbreviations in the art. Each brand and abbreviation is clear and definite in the field of its related use. Those skilled in the art can purchase them from the market or prepare them by conventional methods according to the brands, abbreviations and corresponding uses.
[0032] Preparation Example 1
[0033] 0.3 g of graphene oxide was mixed with 70 mL of deionized water, and ultrasonically dispersed at 300 W for 30 min to collect the dispersion;
[0034] The dispersion was mixed with a 2% by mass diaminoguanidine hydrochloride solution and 0.3-0.5 mL of glutaraldehyde was added. The pH was adjusted to 10.0 with a 0.1% by mass sodium hydroxide solution, and then treated in a water bath at 30° C. for 2 h. The modified dispersion 1 was prepared by ultrasonic dispersion at 200 W.
[0035] Preparation Example 2
[0036] 0.4 g of graphene oxide was mixed with 85 mL of deionized water, and ultrasonically dispersed at 300 W for 30 min to collect the dispersion;
[0037] The dispersion was mixed with a 2% by mass diaminoguanidine hydrochloride solution and 0.4 mL of glutaraldehyde was added. The pH was adjusted to 10.0 with a 0.1% by mass sodium hydroxide solution, and then treated in a water bath at 35° C. for 2 h. The modified dispersion 2 was prepared by ultrasonic dispersion at 200 W.
[0038] Preparation Example 3
[0039] 0.5 g of graphene oxide was mixed with 100 mL of deionized water, and ultrasonically dispersed at 300 W for 30 min to collect the dispersion;
[0040] The dispersion was mixed with a 2% by mass diaminoguanidine hydrochloride solution and 0.5 mL of glutaraldehyde was added. The pH was adjusted to 10.0 with a 0.1% by mass sodium hydroxide solution, and then treated in a water bath at 40° C. for 2 h. The modified dispersion 3 was prepared by ultrasonic dispersion at 200 W.
[0041] Example 1
[0042] Take 35 kg of polyethylene glycol, 5 kg of acetic acid and 500 kg of water, stir and mix, and collect the mixed liquid;
[0043] After adding tetramethoxysilane to the mixed solution, the mixture was stirred at low temperature at 0°C and placed in a water bath, and then stirred and aged for 24 hours in a water bath at 35°C, and a wet silica gel column was collected. The wet silica gel column was treated with 1.5 mol / L ammonia water to collect a silica gel column;
[0044] The silica gel column is sequentially placed in a 0.5 mol / L nitric acid solution, water and N, N-dimethylformamide for immersion and washing for 45 minutes each, then dried at 60°C and calcined at 650°C, allowed to stand and cool, and then immersed in a 2 mol / L hydrochloric acid solution and heated to 80°C, kept warm for 24 hours, and rinsed with deionized water until the washing liquid is neutral, thereby preparing the high-efficiency silica gel monolithic column for refining 2-amino-5-bromopyridine.
[0045] Example 2
[0046] Take 40 kg of polyethylene glycol, 8 kg of acetic acid and 550 kg of water, stir and mix, and collect the mixed liquid;
[0047] After adding tetramethoxysilane to the mixed solution, the mixture was stirred at low temperature at 0°C and placed in a water bath, and then stirred and aged for 24 hours in a 40°C water bath environment, and a wet silica gel column was collected. The wet silica gel column was treated with 1.5 mol / L ammonia water to collect a silica gel column;
[0048] The silica gel column is sequentially placed in a 0.5 mol / L nitric acid solution, water and N, N-dimethylformamide for immersion and washing for 52 minutes each, then dried at 60°C and calcined at 700°C, allowed to stand and cool, and then immersed in a 2 mol / L hydrochloric acid solution and heated to 80°C, kept warm for 24 hours, and rinsed with deionized water until the washing liquid is neutral, thereby preparing the high-efficiency silica gel monolithic column for refining 2-amino-5-bromopyridine.
[0049] Example 3
[0050] Take 45 kg of polyethylene glycol, 10 kg of acetic acid and 600 kg of water, stir and mix, and collect the mixed liquid;
[0051] After adding tetramethoxysilane to the mixed solution, the mixture was stirred at low temperature at 0°C and placed in a water bath, and then stirred and aged for 24 hours in a water bath at 45°C, and a wet silica gel column was collected. The wet silica gel column was treated with 1.5 mol / L ammonia water to collect a silica gel column;
[0052] The silica gel column is sequentially placed in a 0.5 mol / L nitric acid solution, water and N, N-dimethylformamide for immersion and washing for 60 minutes each, then dried at 60°C and calcined at 750°C, allowed to stand and cool, and then immersed in a 2 mol / L hydrochloric acid solution and heated to 80°C, kept warm for 24 hours, and rinsed with deionized water until the washing liquid is neutral, thereby preparing the high-efficiency silica gel monolithic column for refining 2-amino-5-bromopyridine.
[0053] Example 4
[0054] Take 40 kg of polyethylene glycol, 8 kg of acetic acid and 550 kg of water, stir and mix, and collect the mixed liquid;
[0055] After adding tetramethoxysilane to the mixed solution, the mixture was stirred at low temperature at 0°C and placed in a water bath, and then stirred and aged for 24 hours in a 40°C water bath environment, and a wet silica gel column was collected. The wet silica gel column was treated with 1.5 mol / L ammonia water to collect a silica gel column;
[0056] The silica gel column is sequentially placed in a 0.5 mol / L nitric acid solution, water and N, N-dimethylformamide, each soaked and washed for 52 minutes, then dried at 60°C and calcined at 700°C, allowed to stand and cool, and then immersed in a 2 mol / L hydrochloric acid solution, heated to 80°C, and kept warm for 24 hours, and rinsed with deionized water until the washing liquid is neutral, thereby preparing the high-efficiency silica gel monolithic column for purifying 2-amino-5-bromopyridine;
[0057] Take the modified dispersion 1 and place it under ultrasonic dispersion treatment at 200W, then inject it into the high-efficiency silica gel monolithic column for refining 2-amino-5-bromopyridine at 30μL / min, cap it and place it at 38°C for insulation reaction, refine it and cool it to room temperature, rinse it with deionized water and methanol in turn, and dry it to complete the extraction enrichment modification treatment.
[0058] Example 5
[0059] Take 40 kg of polyethylene glycol, 8 kg of acetic acid and 550 kg of water, stir and mix, and collect the mixed liquid;
[0060] After adding tetramethoxysilane to the mixed solution, the mixture was stirred at low temperature at 0°C and placed in a water bath, and then stirred and aged for 24 hours in a 40°C water bath environment, and a wet silica gel column was collected. The wet silica gel column was treated with 1.5 mol / L ammonia water to collect a silica gel column;
[0061] The silica gel column is sequentially placed in a 0.5 mol / L nitric acid solution, water and N, N-dimethylformamide, each soaked and washed for 52 minutes, then dried at 60°C and calcined at 700°C, allowed to stand and cool, and then immersed in a 2 mol / L hydrochloric acid solution, heated to 80°C, and kept warm for 24 hours, and rinsed with deionized water until the washing liquid is neutral, thereby preparing the high-efficiency silica gel monolithic column for purifying 2-amino-5-bromopyridine;
[0062] Take the modified dispersion 2 and place it under ultrasonic dispersion treatment at 200W, then inject it into the high-efficiency silica gel monolithic column for refining 2-amino-5-bromopyridine at 30μL / min, cap it and place it at 40°C for insulation reaction. After refining and cooling to room temperature, rinse it with deionized water and methanol in turn, and dry it to complete the extraction enrichment modification treatment.
[0063] Example 6
[0064] Take 40 kg of polyethylene glycol, 8 kg of acetic acid and 550 kg of water, stir and mix, and collect the mixed liquid;
[0065] After adding tetramethoxysilane to the mixed solution, the mixture was stirred at low temperature at 0°C and placed in a water bath, and then stirred and aged for 24 hours in a 40°C water bath environment, and a wet silica gel column was collected. The wet silica gel column was treated with 1.5 mol / L ammonia water to collect a silica gel column;
[0066] The silica gel column is sequentially placed in a 0.5 mol / L nitric acid solution, water and N, N-dimethylformamide, each soaked and washed for 52 minutes, then dried at 60°C and calcined at 700°C, allowed to stand and cool, and then immersed in a 2 mol / L hydrochloric acid solution, heated to 80°C, and kept warm for 24 hours, and rinsed with deionized water until the washing liquid is neutral, thereby preparing the high-efficiency silica gel monolithic column for purifying 2-amino-5-bromopyridine;
[0067] Take the modified dispersion 3 and place it under ultrasonic dispersion treatment at 200W, then inject it into the high-efficiency silica gel monolithic column for refining 2-amino-5-bromopyridine at 30μL / min, cap it and place it at 45°C for insulation reaction. After refining and cooling to room temperature, rinse it with deionized water and methanol in turn, and dry it to complete the extraction enrichment modification treatment.
[0068] Performance testing
[0069] The 2-amino-5-bromopyridine prepared in Example 1-6 was purified and detected by a high-efficiency silica gel monolithic column through an electrochromatographic experiment.
[0070] The total length of the chromatographic column is 33.5 cm and the effective length is 25 cm. The polyimide coating is removed at the end of the stationary phase of the high-efficiency silica gel monolithic column for 2-amino-5-bromopyridine purification. 2-amino-5-bromopyridine is subjected to chromatographic separation.
[0071] The specific test data are shown in Table 1.
[0072] Table 1 Performance test table
[0073]
[0074]
[0075] Based on the data of Examples 1-6, analysis and explanation are provided.
[0076] It can be seen from Table 1 and Examples 1-3 that the present application optimizes the preparation process of the silica gel monolithic column. The present application adopts an aqueous ammonia solution as a pore-forming agent and optimizes the solubility of aqueous ammonia so that the silica gel monolithic column prepared in the present application has an excellent dual-pore structure of macropores and mesopores, thereby improving the defect of poor separation efficiency of a single pore size, thereby effectively improving the refining efficiency of 2-amino-5-bromopyridine.
[0077] As can be seen from Table 1 and Examples 4-6, the present application uses amino-modified graphene oxide material as the main modified material to modify the silica gel monolithic column. Since the graphene oxide material is a material of a two-dimensional spatial structure and contains rich functional groups such as hydroxyl and carboxyl, the silica gel monolithic column can be effectively modified and modified. At the same time, in the amino-modified graphene oxide material, the amino-modified material can react with the carboxyl amidation of the graphene surface to improve the roughness and specific surface area of the graphene oxide material, thereby further improving the enrichment performance of the silica gel monolithic column material and the chromatographic separation performance of 2-amino-5-bromopyridine. This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. After reading this specification, those skilled in the art can make modifications to the present embodiment without creative contributions as needed, but as long as they are protected by the patent law within the scope of the claims of the present application.
Claims
1. A method for preparing a high-efficiency silica gel monolithic column for refining 2-amino-5-bromopyridine, It is characterized in that The method comprises the following preparation steps: Take polyethylene glycol, acetic acid and water, stir and mix, and collect the mixed solution; After adding tetramethoxysilane to the mixed solution, stirring at low temperature and placing in a water bath, stirring and aging in a water bath environment, collecting a wet silica gel column, taking the wet silica gel column and treating it with 1.5 mol / L ammonia water to collect a silica gel column; The silica gel column is immersed in washing treatment, dried and then calcined, left to cool and immersed in a hydrochloric acid solution, and washed with water until neutral, so as to prepare the high-efficiency silica gel monolithic column for purifying 2-amino-5-bromopyridine.
2. A method for preparing a high-efficiency silica gel monolithic column for refining 2-amino-5-bromopyridine according to claim 1, It is characterized in that The immersion solutions used in the immersion washing treatment are nitric acid solution, water and N,N-dimethylformamide in sequence.
3. A method for preparing a high-efficiency silica gel monolithic column for refining 2-amino-5-bromopyridine according to claim 1, It is characterized in that The addition ratio of the polyethylene glycol, acetic acid and water is (7-10):1:(100-120).
4. A method for preparing a high-efficiency silica gel monolithic column for refining 2-amino-5-bromopyridine according to claim 1, It is characterized in that It also includes an extraction enrichment modification process, wherein the extraction enrichment modification process includes the following steps: The modified dispersion was subjected to ultrasonic dispersion treatment and then injected into a high-efficiency silica gel monolithic column for 2-amino-5-bromopyridine purification at 30 μL / min. After end-capping, the column was placed at 38-45°C for heat preservation and reaction. After purification and cooling to room temperature, the column was rinsed with deionized water and methanol in turn and dried to complete the extraction, enrichment and modification treatment.
5. A method for preparing a high-efficiency silica gel monolithic column for refining 2-amino-5-bromopyridine according to claim 4, It is characterized in that The modified dispersion is amino-modified graphene oxide.
6. A method for preparing a high-efficiency silica gel monolithic column for purifying 2-amino-5-bromopyridine according to claim 4, It is characterized in that The modified dispersion is prepared by the following scheme: Graphene oxide and deionized water are stirred and mixed, and a dispersion is collected by ultrasonic dispersion; The modified dispersion is prepared by mixing the dispersion and diaminoguanidine hydrochloride, adding glutaraldehyde, adjusting the pH to 10.0, treating the mixture in a water bath, and performing ultrasonic dispersion.
7. A method for preparing a high-efficiency silica gel monolithic column for purifying 2-amino-5-bromopyridine according to claim 6, It is characterized in that The water bath treatment temperature is 30-40°C.
Citation Information
Patent Citations
Preparation method of hybridized silica gel monolithic column
CN104258805A
Affine monolithic column based on graphene-nanogold composite interface for highly supporting aptamer and preparation method of affine monolithic column
CN110215737A