Granulation method of micro-fine-particle artificial rutile
By using a mixture of alkali metal carbonate and sulfate as a binder, fine-grained artificial rutile with a particle size meeting the requirements of boiling chlorination furnaces is prepared, which solves the problems of excessive particle size and impurities introduced by the binder in the prior art, and realizes the problem of excessive particle size and the introduction of impurities in the binder. It has high efficiency granulation and good thermal stability, and meets the needs of boiling chlorination process.
Patent Information
- Application Number
- CN202411256331.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, fine-grained artificial rutile cannot meet the particle size requirements of the boiling chlorination process, resulting in insufficient contact between titanium-rich material and chlorine gas in the boiling chlorination furnace, reducing the chlorination reaction rate, and commonly used binders are under high temperature environments. It is easy to introduce impurities and affect product quality.
A mixture of alkali metal carbonate and alkali metal sulfuric acid salt is used as a binder, and is arranged as a binder solution with water, sprayed on finely pelletized artificial rutile, and produced in a wet high-speed stirring granulator The particles were then dried in a fluidized bed to prepare particles with a particle size distribution of 96-900 μm, with good cold strength and thermal stability.
It has achieved fine-grained artificial rutile with high granulation efficiency, high product quality and low cost, meeting the requirements of boiling chlorination process, and improving the utilization rate of titanium resources and the production capacity of high-end titanium products.
Smart Images

Figure BDA0005034203240000041
Abstract
Description
Technical Field
[0001] The invention belongs to the field of nonferrous metal metallurgy, and in particular relates to a granulation method of fine-grained artificial rutile. Background Art
[0002] Titanium is an important strategic metal in my country and has important applications in aerospace, navigation, military industry, daily chemical industry and other fields. The main products of the titanium industry are titanium dioxide, titanium metal and titanium alloys. About 95% of the world's titanium resources are used to produce titanium dioxide. The boiling chlorination method has simple production equipment, large titanium tetrachloride output, and low three waste emissions. It is the mainstream process for the production of titanium dioxide by the chlorination method in my country. The boiling chlorination method requires that the calcium and magnesium impurity content of the raw materials entering the furnace is less than 1.5%, of which CaO is less than 0.14%, and the titanium grade is ≥90%. The boiling chlorination furnace is a fluidized bed system. In order to ensure that the titanium-rich material always maintains a fluidized state in the boiling chlorination furnace, the particle size distribution of the raw materials entering the furnace is required to be between 96μm and 900μm.
[0003] my country's titanium resources are mainly found in ilmenite, usually 40-45%. In order to make ilmenite meet the production requirements of boiling chlorination method, it needs to be enriched into high-grade titanium-rich materials (artificial rutile, high-titanium slag). Artificial rutile has advantages in product quality and performance structure, and plays an important role in high-end titanium products. my country's ilmenite contains a lot of calcium and magnesium impurities, which need to be removed by grinding and acid leaching to obtain artificial rutile, but the product particle size is basically less than 100μm. Therefore, domestic artificial rutile has the problem of too fine particles and is difficult to be applied to boiling chlorination process.
[0004] In order to increase the particle size of artificial rutile and make it meet the requirements of boiling chlorination process, researchers selected various types of binders to granulate artificial rutile. Granulation binders can be divided into three categories: organic binders, inorganic binders and composite binders. Organic binders have a good bonding effect on artificial rutile under low temperature conditions, but they are expensive and have poor thermal stability. They will decompose rapidly in the high temperature environment of the boiling chlorination furnace, causing the artificial rutile particles to scatter and reduce the chlorination efficiency. Inorganic binders can maintain the complete morphology of artificial rutile granules under high temperature conditions, but it is easy to introduce a variety of impurity elements when selecting inorganic binders: impurity elements such as Ca and Mg will react with chlorine in the boiling chlorination furnace to generate high-boiling point chlorides, which exist in liquid form in a reaction environment of 900-1100℃, causing the materials to stick together and agglomerate, destroying the stability of the bed; impurity elements such as P and V will react with chlorine in the boiling chlorination furnace to generate chloride impurities with a boiling point similar to TiCl4, which are difficult to separate from TiCl4 and affect the quality of TiCl4. Composite adhesives are a combination of multiple adhesives, making full use of the advantages of each adhesive, but the amount of adhesive used is prone to increase, introducing multiple impurities.
[0005] Since the particle size of artificial rutile particles less than 100 μm is too small, the relative force between particles is large, which easily leads to the agglomeration of material particles during the boiling chlorination process, forming channel flow and slugging phenomena, resulting in insufficient contact between the titanium-rich material and chlorine in the furnace, reducing the chlorination reaction rate, and causing large particle escape, high dust collection pressure of the boiling chlorination furnace, large proportion of mud in the titanium tetrachloride product, and increased slag production. Therefore, it is necessary to prepare it into particles that meet the particle size requirements of the boiling chlorination furnace through a granulation process.
[0006] By improving the granulation process, artificial rutile particles that meet the requirements of the boiling chlorination furnace can be prepared and have good cold strength and thermal stability. This is of great significance to the full utilization of titanium resources and the development of high-end titanium product production in my country. Summary of the invention
[0007] In view of the problem in the prior art that "fine-grained artificial rutile cannot meet the requirements of the boiling chlorination process", the purpose of the present invention is to provide a granulation method for fine-grained artificial rutile, which has the characteristics of high granulation efficiency, high product quality and low cost, and can meet the requirements of the boiling chlorination process.
[0008] In order to achieve the above object, the present invention provides a method for granulating fine-grained artificial rutile, comprising the following steps:
[0009] (1) preparing a binder: weighing a binder and water according to a set ratio and mixing them evenly to prepare a binder solution, wherein the binder is one or a combination of alkali metal carbonate and alkali metal sulfuric acid salt;
[0010] (2) Raw material mixing: spraying the prepared binder solution evenly on the fine-grained artificial rutile and mixing evenly to obtain a mixed raw material;
[0011] (3) Granulation: placing the mixed raw materials in a granulator for granulation;
[0012] (4) Drying and solidification: The granulated product is dried and solidified to obtain.
[0013] The micro-grained artificial rutile described in the present invention is a material with a particle size of less than 100 μm after chemical treatment.
[0014] In step (1), the amount of binder added is 0.5-3% of the mass of the fine-grained artificial rutile; and the amount of water added is 10-30% of the mass of the fine-grained titanium-rich material.
[0015] In step (2), fine-grained artificial rutile and a binder are mixed uniformly.
[0016] In step (3), the granulation equipment used is a wet high-speed stirring granulator.
[0017] In step (3), the stirring blade speed is set to 200-600 rpm, the cutting blade speed is set to 500-2000 rpm, and the granulation time is set to 2-10 minutes.
[0018] In step (4), the granulated product particles are placed in a fluidized bed dryer for drying. The fine particles carried out by the airflow during the drying process and the coarse particles that settle down are collected and returned to the ingredients in step (2); the material stabilized in the fluidized bed is a qualified product after drying, and the qualified particle size is 96μm to 900μm.
[0019] The binder used in the present invention is one or a mixture of alkali metal carbonate, alkali metal sulfuric acid salt, which reacts with chlorine gas under boiling chlorination process conditions to generate corresponding chloride impurities, such as NaCl, KCl and SO2, etc. Alkali metal chlorides such as NaCl and KCl are high-boiling point substances, but they are easily volatile at the boiling chlorination reaction temperature and have little effect on the fluidized environment in the boiling chlorination furnace.
[0020] Compared with the prior art, the beneficial technical effects of the present invention are:
[0021] 1) The present invention provides a method for granulating fine-grained artificial rutile, wherein an alkali metal carbonate, an alkali metal sulfate acid salt, or a mixture of the two is prepared with water to form a binder solution, and artificial rutile particles smaller than 100 μm are placed in a high-speed stirring granulator for uniform mixing, and the material with a particle size distribution of 96 to 900 μm accounts for more than 90%, and has good strength, and can be used in a boiling chlorination furnace. This granulation method has a high pass rate, a simple granulation process, and is environmentally friendly.
[0022] 2) In patent CN 202210349625.3, ferrous sulfate and silica sol are selected as binders to granulate fine-grained titanium-rich material. The cold strength of the product particles is 13.94% and 16.37%, respectively, and the hot strength is 5.44% and 7.30%, respectively. The strength is worse than the binder granulation product proposed in the present invention.
[0023] 3) Patent CN 202210349636.1 is aimed at granulation raw materials that are titanium-rich materials (fine-grained high-titanium slag, fine-grained artificial rutile, and natural rutile). The surface properties of fine-grained high-titanium slag and fine-grained artificial rutile are significantly different. The surface properties of high-titanium slag are active and easier to bond with the binder, while the properties of artificial rutile are more stable. According to the experiment of Comparative Example 3, the binder aluminum sulfate used has limited effect on fine-grained artificial rutile, and the granulation rate is only 46.78%, which is much lower than the binder provided by the present invention.
[0024] 4) The present invention uses an inorganic binder. Compared with the composite organic binder of 60% to 70% heavy oil, 5% to 15% sodium cellulose and 20% to 30% dextrin selected in CN 201510736993.3, the binder of the present invention has a lower dosage, better thermal stability, and no corrosive substances are generated during the boiling chlorination reaction. Therefore, the binder of the present invention is more suitable for boiling chlorination industrial production. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0026] The present invention provides a fine-grained artificial rutile granulation binder, which is prepared by using an alkali metal carbonate, an alkali metal sulfate acid salt or a mixture of the two and water to form a binder solution, and the prepared binder solution is sprayed on artificial rutile particles less than 100 μm and mixed evenly. The mixed material is pre-treated by a high-pressure roller mill and then placed in a wet high-speed stirring granulator for granulation treatment, and the product particles obtained by granulation are subjected to fluidized bed drying treatment. The cold strength and hot strength of particles with a particle size distribution between 96 and 900 μm are measured.
[0027] In the present invention, the cold strength and hot strength of the granulated product are tested. The heat treatment method of the product particles is carried out in a muffle furnace by a coke burying method. 200g of dry granular products with a particle size distribution of 96-900μm are weighed each time, placed in a Φ10×13cm graphite crucible and wrapped with coke powder (particle size greater than 3mm, washed until there is no micropowder particles on the surface and completely dried), placed in a muffle furnace, heated to 1000°C with the furnace, and taken out after 60 minutes for measuring its hot strength.
[0028] The present invention adopts the method of measuring the wear index of the granulated product as the cold and hot strength characterization method of the granulated product. The present invention adopts the reduction pulverization drum to detect the wear index of the product granules, the drum size is Φ130×200mm, the speed is 30 rpm, and the time is 10 minutes. Each time, 100g of granular materials distributed in 96-900μm are weighed for the experiment, and the arithmetic mean value is taken as the wear index RDI after repeating 3 times.
[0029]
[0030] Where: m D0 —The mass of the sample before drum rotation;
[0031] m D1 —Mass after drumming +0.096mm.
[0032] The process of the present invention is described below in conjunction with specific embodiments.
[0033] Example 1
[0034] Weigh 20g of anhydrous sodium carbonate and put it into 100g of water to prepare a binder solution for standby use. Weigh 1000g of fine-grained artificial rutile (particle size less than 100μm) and mix it evenly with the binder, place it in a wet high-speed stirring granulator, set the stirring paddle speed to 400rpm, the cutting knife speed to 1000rpm, and the granulation time to 6 minutes. The granulated product particles are placed in a fluidized bed dryer for drying, and the particle size distribution is between 96 and 900μm, accounting for 74.34%, the particle 105℃ drying strength wear index is 8.54%, and the particle 1000℃ thermal strength wear index is 4.40%.
[0035] Example 2
[0036] Weigh 30g of anhydrous potassium carbonate and put it into 100g of water to prepare a binder solution for standby use. Weigh 1000g of fine-grained artificial rutile (particle size less than 100μm) and mix it evenly with the binder, place it in a wet high-speed stirring granulator, set the stirring paddle speed to 400rpm, the cutting knife speed to 2000rpm, and the granulation time to 6 minutes. The granulated product particles are placed in a fluidized bed dryer for drying, and the particle size distribution is between 96 and 900μm, accounting for 77.35%, the particle cold strength wear index is 11.46%, and the particle hot strength wear index is 5.04%.
[0037] Example 3
[0038] Weigh 10g of sodium bisulfate and put it into 200g of water to prepare a binder solution for standby use. Weigh 1000g of fine-grained artificial rutile (particle size less than 100μm) and mix it evenly with the binder, place it in a wet high-speed stirring granulator, set the stirring paddle speed to 500rpm, the cutting knife speed to 1000rpm, and the granulation time to 6 minutes. The granulated product particles are placed in a fluidized bed dryer for drying, and the particle size distribution obtained is between 96 and 900μm, accounting for 83.35%. The cold strength wear index of qualified particles is 1.51%, and the hot strength wear index is 1.04%.
[0039] Example 4
[0040] Weigh 5g of potassium bisulfate and put it into 300g of water to prepare a binder solution for standby use. Weigh 1000g of fine-grained artificial rutile (particle size less than 100μm) and mix it evenly with the binder, place it in a wet high-speed stirring granulator, set the stirring paddle speed to 200rpm, the cutting knife speed to 500rpm, and the granulation time to 10 minutes. The granulated product particles are placed in a fluidized bed dryer for drying, and the particle size distribution is between 96 and 900μm, accounting for 78.65%, the particle 105℃ drying strength wear index is 1.62%, and the particle 1000℃ thermal strength wear index is 1.23%.
[0041] Example 5
[0042] Weigh 10g of potassium hydrogen sulfate and put it into 200g of water to prepare a binder solution for standby use. Weigh 1000g of fine-grained artificial rutile (particle size less than 100μm) and mix it evenly with the binder, place it in a wet high-speed stirring granulator, set the stirring paddle speed to 600rpm, the cutting knife speed to 1500rpm, and the granulation time to 8 minutes. The granulated product particles are placed in a fluidized bed dryer for drying, and the particle size distribution is between 96 and 900μm, accounting for 80.23%, the particle 105℃ drying strength wear index is 1.78%, and the particle 1000℃ thermal strength wear index is 1.29%.
[0043] Example 6
[0044] Weigh 10g of anhydrous sodium carbonate and 10g of sodium bisulfate and put them into 200g of water to prepare a binder solution for standby use. Weigh 1000g of fine-grained artificial rutile (particle size less than 100μm) and mix it evenly with the binder, place it in a wet high-speed stirring granulator, set the stirring paddle speed to 600rpm, the cutting knife speed to 1500rpm, and the granulation time to 8 minutes. The granulated product particles are placed in a fluidized bed dryer for drying, and the particle size distribution is between 96 and 900μm, accounting for 79.65%, the particle 105℃ drying strength wear index is 5.22%, and the particle 1000℃ thermal strength wear index is 3.26%.
[0045] Example 7
[0046] Weigh 20g of anhydrous sodium carbonate and 10g of sodium bisulfate and put them into 200g of water to prepare a binder solution for standby use. Weigh 1000g of fine-grained artificial rutile (particle size less than 100μm) and mix it evenly with the binder, place it in a wet high-speed stirring granulator, set the stirring paddle speed to 600rpm, the cutting knife speed to 1500rpm, and the granulation time to 8 minutes. The granulated product particles are placed in a fluidized bed dryer for drying, and the particle size distribution is between 96 and 900μm, accounting for 81.36%, the particle 105℃ drying strength wear index is 5.01%, and the particle 1000℃ thermal strength wear index is 4.23%.
[0047] Comparative Example 1
[0048] Weigh 30g of ferrous sulfate and put it into 200g of water to prepare a binder solution for standby use. Weigh 1000g of fine-grained artificial rutile (particle size less than 100μm) and mix it evenly with the binder, place it in a wet high-speed stirring granulator, set the stirring paddle speed to 400rpm, the cutting knife speed to 1000rpm, and the granulation time to 6 minutes. The granulated product particles are placed in a fluidized bed dryer for drying, and the particle size distribution is between 96 and 900μm, accounting for 46.35%. Using ferrous sulfate as a granulation binder, the granulation effect of fine-grained artificial rutile is poor.
[0049] Comparative Example 2
[0050] Weigh 30g of silica sol and put it into 200g of water to prepare a binder solution for standby use. Weigh 1000g of fine-grained artificial rutile (particle size less than 100μm) and mix it evenly with the binder, place it in a wet high-speed stirring granulator, set the stirring paddle speed to 400rpm, the cutting knife speed to 1000rpm, and the granulation time to 6 minutes. The granulated product particles are placed in a fluidized bed dryer for drying, and the particle size distribution obtained is between 96 and 900μm, accounting for 32.96%. The granulation efficiency of fine-grained artificial rutile is poor.
[0051] Comparative Example 3
[0052] Weigh 30g of aluminum sulfate and put it into 200g of water to prepare a binder solution for standby use. Weigh 1000g of fine-grained artificial rutile (particle size less than 100μm) and mix it evenly with the binder, place it in a wet high-speed stirring granulator, set the stirring paddle speed to 400rpm, the cutting knife speed to 1000rpm, and the granulation time to 6 minutes. The granulated product particles are placed in a fluidized bed dryer for drying, and the particle size distribution obtained is between 96 and 900μm, accounting for 46.78%. The granulation efficiency of fine-grained artificial rutile is poor.
[0053] The granulation method of the present invention provides a fine-grained artificial rutile granulation binder, which has high granulation efficiency, good product quality, low cost, and is easy to store and transport. It effectively solves the problem that fine-grained artificial rutile is difficult to be used in a boiling chlorination furnace to prepare titanium tetrachloride due to its too fine particles.
[0054] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. For those skilled in the art, improvements and changes obtained without departing from the technical concept of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A method for granulating fine-grained artificial rutile, It is characterized in that The following steps are involved: (1) preparing a binder: weighing a binder and water according to a set ratio and mixing them evenly to prepare a binder solution, wherein the binder is one or a combination of alkali metal carbonate and alkali metal sulfuric acid salt; (2) Raw material mixing: spraying the prepared binder solution evenly on the fine-grained artificial rutile and mixing evenly to obtain a mixed raw material; (3) Granulation: placing the mixed raw materials in a granulator for granulation; (4) Drying and solidification: The granulated product is dried and solidified to obtain.
2. The method for granulating fine-grained artificial rutile according to claim 1, It is characterized in that The micro-grained artificial rutile is a material with a particle size less than 100 μm after chemical treatment.
3. The method for granulating fine-grained artificial rutile according to claim 1, It is characterized in that In step (1), the amount of binder added is 0.5-3% of the mass of the fine-grained artificial rutile; and the amount of water added is 10-30% of the mass of the fine-grained titanium-rich material.
4. The method for granulating fine-grained artificial rutile according to claim 1, It is characterized in that In step (3), the granulation equipment used is a wet high-speed stirring granulator.
5. The method for granulating fine-grained artificial rutile according to claim 4, It is characterized in that The stirring blade speed is set to 200-600 rpm, the cutting blade speed is set to 500-2000 rpm, and the granulation time is set to 2-10 minutes.
6. The method for granulating fine-grained artificial rutile according to claim 1, It is characterized in that In step (4), the granulated product particles are placed in a fluidized bed dryer for drying. The fine particles carried out by the airflow during the drying process and the coarse particles that settle down are collected and returned to the ingredients in step (2); the material stabilized in the fluidized bed is a qualified product after drying, and the qualified particle size is 96μm to 900μm.
Citation Information
Cited By
Granulation method of fine-fraction titanium-rich material
CN121629188A