Reusable filter aid for dewatering fluorine-containing sludge and preparation method thereof

The magnetic iron tetraoxide nanoparticle filter aid modified by alkyl carboxylic acid solves the problem of high moisture content of fluorine-containing sludge and difficult to reuse the filter aid, achieving efficient dehydration and reusable resources.

CN119034687AActive Publication Date: 2024-11-29GUOFU NEW MATERIALS (GUANGDONG) CO LTD

Patent Information

Application Number
CN202411187818.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-07-19
Filing Date
2024-08-28
Publication Date
2024-11-29
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The prior art is difficult to effectively deal with the high moisture content of fluorine-containing sludge, resulting in high cost of sludge disposal and drying, and it is difficult to reuse ordinary filter aids, resulting in waste of resources and secondary pollution.

Method used

Magnetic ferrotetraoxide nanoparticles modified with alkyl carboxylic acid are prepared by co-precipitation method, amino modification and alkyl carboxylic acid modification treatment, and provide a magnetic carrier to solidly support the surfactant. , used for filtering and dehydration of fluorine-containing sludge.

Benefits of technology

The filtration time is significantly shortened, the moisture content of the sludge filter cake is reduced, and the filter aid is easy to separate and reused, maintaining efficient dehydration performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005014044250000051
    Figure BDA0005014044250000051
  • Figure BDA0005014044250000061
    Figure BDA0005014044250000061
Patent Text Reader

Abstract

The invention relates to a reusable filter aid for filtering and dewatering fluorine-containing sludge and a preparation method of the reusable filter aid in order to solve the technical problems that fluorine-containing sludge is difficult to dewater, common chemical filter aids are difficult to recycle and the like at the same time, and the invention relates to the reusable filter aid for filtering and dewatering the fluorine-containing sludge and the preparation method of the reusable filter aid. The preparation method comprises the following three steps: (1) preparing magnetic ferroferric oxide nano-particles by adopting a coprecipitation method; (2) performing surface amino modification on the magnetic ferroferric oxide nano-particles; and (3) performing alkyl carboxylic acid modification on the magnetic ferroferric oxide nano-particles. Compared with the prior art, the invention has the advantages of simple preparation method, excellent filtration aiding effect (obviously shortened filtration time and obviously reduced water content of sludge filter cake), stable reuse performance and the like, and has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the solid-liquid separation of fluorine-containing sludge and purified water generated in the process of treating fluorine-containing wastewater by a precipitation method, and in particular to a reusable filter aid in the process of filtering and dehydrating fluorine-containing sludge and a preparation method thereof. Background Art

[0002] In the etching process of solar cell and chip preparation, a large amount of hydrofluoric acid is used and the fluorine-containing etching solution produced is a typical type of fluorine-containing wastewater. In recent years, with the rapid development of photovoltaic power generation industry and semiconductor industry, the discharge of this fluorine-containing wastewater has also increased year by year. In addition, fluorine chemical industry, non-ferrous metal smelting, glass and silicon-containing electronic components are also important sources of fluorine-containing wastewater. As the main source of fluorine pollution in the environment, the fluorine element dispersed in the water body is extremely harmful and is an important safety hazard for maintaining the stability of the ecological environment and the healthy development of human society. Under the severe situation, the removal of fluorine in fluorine-containing wastewater has also been a key research object of the environmental protection industry in recent years. Among the many fluorine-containing wastewater treatment methods, calcium ion precipitation method, coagulation precipitation method and adsorption method are three typical high-efficiency and low-consumption methods, which are also the treatment methods commonly used in industry. By cleverly combining the above three treatment methods, wastewater with different fluorine contents can be widely treated. The treated water can meet the national first-level wastewater discharge standard, and most of the fluorine elements are transferred to the fluorine-containing sludge.

[0003] Calcium fluoride in fluoride-containing sludge is an important fluorine regeneration resource. There have been many literature reports on the purification of calcium fluoride from fluoride-containing sludge. In order to utilize calcium fluoride in fluoride-containing sludge, the first problem to be faced is to separate fluoride-containing sludge from treated wastewater. At present, the main means of separating fluoride-containing sludge and purified water in industry is the plate and frame filter press process. Fluoride-containing sludge contains not only calcium salt precipitates represented by calcium fluoride, calcium carbonate, and calcium sulfate, but also various flocculant colloids with strong hydrophilicity. Through plate and frame filter press separation, the moisture content of the filter cake obtained by treating fluoride-containing wastewater from different factories is generally above 50%, and some are as high as about 75%. The high moisture content of fluoride-containing sludge undoubtedly increases the cost of sludge disposal, transportation cost, and subsequent drying energy consumption. Considering the economic and energy consumption issues, it is very necessary to explore low-energy and high-efficiency methods for dehydrating fluoride-containing sludge. Similar to the enhanced dehydration method of other industrial sludge, adding filter aids during the filtration process is considered to be the simplest and most effective method. However, common physical filter aids such as diatomaceous earth and volcanic ash are likely to remain in fluoride-containing sludge, making subsequent calcium fluoride purification more difficult; chemical filter aids such as various surfactants are likely to be lost into the treated clean water, causing secondary pollution. Therefore, how to construct an efficient, easily recyclable and reusable filter aid is one of the important problems that should be solved at present. Summary of the invention

[0004] The present invention provides a reusable filter aid for dehydrating fluorine-containing sludge and a preparation method thereof, so as to simultaneously solve the technical problems of difficulty in dehydrating fluorine-containing sludge and difficulty in recycling common chemical filter aids, and realize efficient dehydration of fluorine-containing sludge.

[0005] In order to solve the above problems, the present invention discloses a reusable filter aid for filtering and dehydrating fluorine-containing sludge, characterized in that the main component is alkyl carboxylic acid-modified magnetic ferrosoferric oxide nanoparticles.

[0006] The present invention also discloses a method for preparing the above-mentioned reusable filter aid for filtering and dehydrating fluorine-containing sludge, which is carried out according to the following steps:

[0007] (1) Preparation of magnetic FeO4 nanoparticles by coprecipitation method

[0008] Weigh 3.89 g of ferric chloride and 3.34 g of ferrous sulfate heptahydrate and dissolve them in 400 mL of deionized water. Start stirring, heat to 50° C. at 300 rpm, drop 30 mL of 15% sodium hydroxide solution under nitrogen protection, continue crystallization for 1 hour after the dropwise addition, separate the solid product by a magnet, and dry it in an oven at 120° C. for 12 hours to obtain magnetic ferrosoferric oxide nanoparticles;

[0009] (2) Surface amino modification of magnetic FeO nanoparticles

[0010] Weigh 2 g of the magnetic ferroferric oxide nanoparticles prepared in step (1), and evenly disperse them in 200 mL of ethanol by ultrasonication. Then, add 3-aminopropyltriethoxysilane under mechanical stirring, react at 30° C. for 12 hours, separate the solid product with a magnet, wash with ethanol, and dry in an oven at 120° C. for 12 hours to obtain amino-functionalized magnetic ferroferric oxide nanoparticles (hereinafter referred to as amino-functionalized magnetic particles).

[0011] (3) Alkyl carboxylic acid modification of magnetic ferroferric oxide nanoparticles

[0012] Weigh 1 g of the amino magnetic particles obtained in step (2), and evenly disperse them in 100 mL of an organic solvent by ultrasound. Then, add alkyl dicarboxylic acid and a catalyst under mechanical stirring, and react at 120° C. for 24 hours. Collect the solid product by a magnet, wash it with anhydrous ethanol, and dry it in an oven at 120° C. for 12 hours to obtain alkyl carboxylic acid-modified magnetic ferrosoferric oxide nanoparticles.

[0013] In step 2 of the above method, the amount of 3-aminopropyltriethoxysilane used is 0.5g to 1g.

[0014] In step 3 of the above method, the organic solvent is any one of dimethylformamide (DMF), dimethylacetamide, and dimethyl sulfoxide.

[0015] In step 3 of the above method, the alkyl dicarboxylic acid is any one of alkyl dicarboxylic acids with different carbon chain lengths, specifically any one of sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid and octadecanedioic acid.

[0016] In step 3 of the above method, the amount of the alkyl dicarboxylic acid used is 0.2 g to 1 g.

[0017] In step 3 of the above method, the catalyst is 4-dimethylaminopyridine, and its usage is 0.02g to 0.1g.

[0018] The present invention has the following advantages:

[0019] (1) The present invention uses magnetic ferroferric oxide nanoparticles as magnetic carriers for alkyl carboxylic acid surfactants, and immobilizes the alkyl carboxylic acid surfactants on the magnetic nanoparticles through chemical covalent bonds. The preparation method is simple.

[0020] (2) The alkyl carboxylic acid modified magnetic particles prepared by the present invention have excellent filter aid effect in the filtration and dehydration of fluorine-containing sludge (the filtration time is significantly shortened and the moisture content of the sludge filter cake is significantly reduced). In addition, the magnetic filter aid is easy to separate from the fluorine-containing sludge by magnets, and has stable performance in repeated use, and has a good application prospect. DETAILED DESCRIPTION

[0021] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0022] Example 1

[0023] Weigh 3.89 g of ferric chloride and 3.34 g of ferrous sulfate heptahydrate and dissolve them in 400 mL of deionized water. Start stirring and heat to 50° C. at 300 rpm. Add 30 mL of 15% sodium hydroxide solution under nitrogen protection. After the addition, continue crystallization for 1 hour. Separate the solid product by a magnet and dry it in an oven at 120° C. for 2 hours to obtain magnetic ferrosoferric oxide nanoparticles.

[0024] Weigh 2 g of the above-mentioned magnetic ferroferric oxide nanoparticles, uniformly disperse them in 200 mL of ethanol by ultrasound, then add 1 g of 3-aminopropyltriethoxysilane under mechanical stirring, react at 30°C for 12 hours, separate the solid product with a magnet, wash with anhydrous ethanol to remove unreacted 3-aminopropyltriethoxysilane, and dry in an oven at 120°C for 2 hours to obtain amino-terminated functionalized magnetic ferroferric oxide nanoparticles (hereinafter referred to as amino-terminated magnetic particles).

[0025] 1 g of the above-mentioned amino magnetic particles was weighed and uniformly dispersed in 100 mL of organic solvent DMF by ultrasound, and then 0.5 g of decanedicarboxylic acid and 0.05 g of catalyst 4-dimethylaminopyridine were added under mechanical stirring, and the mixture was reacted at 120° C. for 24 hours. The solid product collected by the magnet was washed with anhydrous ethanol and dried in an oven at 120° C. for 2 hours to obtain alkyl carboxylic acid-modified magnetic ferrosoferric oxide nanoparticles.

[0026] Example 2

[0027] Weigh 3.89 g of ferric chloride and 3.34 g of ferrous sulfate heptahydrate and dissolve them in 400 mL of deionized water. Start stirring and heat to 50° C. at 300 rpm. Add 30 mL of 15% sodium hydroxide solution under nitrogen protection. After the addition, continue crystallization for 1 hour. Separate the solid product by a magnet and dry it in an oven at 120° C. for 2 hours to obtain magnetic ferrosoferric oxide nanoparticles.

[0028] Weigh 2 g of the above-mentioned magnetic ferroferric oxide nanoparticles, uniformly disperse them in 200 mL of ethanol by ultrasound, then add 1 g of 3-aminopropyltriethoxysilane under mechanical stirring, react at 30°C for 12 hours, separate the solid product with a magnet, wash with anhydrous ethanol to remove unreacted 3-aminopropyltriethoxysilane, and dry in an oven at 120°C for 2 hours to obtain amino-terminated functionalized magnetic ferroferric oxide nanoparticles (hereinafter referred to as amino-terminated magnetic particles).

[0029] 1 g of the above-mentioned amino magnetic particles was weighed and uniformly dispersed in 100 mL of organic solvent DMF by ultrasound, and then 0.5 g of dodecyl dicarboxylic acid and 0.05 g of catalyst 4-dimethylaminopyridine were added under mechanical stirring, and the mixture was reacted at 120° C. for 24 hours. The solid product collected by the magnet was washed with anhydrous ethanol and dried in an oven at 120° C. for 2 hours to obtain alkyl carboxylic acid-modified magnetic ferrosoferric oxide nanoparticles.

[0030] Example 3

[0031] Weigh 3.89 g of ferric chloride and 3.34 g of ferrous sulfate heptahydrate and dissolve them in 400 mL of deionized water. Start stirring and heat to 50° C. at 300 rpm. Add 30 mL of 15% sodium hydroxide solution under nitrogen protection. After the addition, continue crystallization for 1 hour. Separate the solid product by a magnet and dry it in an oven at 120° C. for 2 hours to obtain magnetic ferrosoferric oxide nanoparticles.

[0032] Weigh 2 g of the above-mentioned magnetic ferroferric oxide nanoparticles, uniformly disperse them in 200 mL of ethanol by ultrasound, then add 1 g of 3-aminopropyltriethoxysilane under mechanical stirring, react at 30°C for 12 hours, separate the solid product with a magnet, wash with anhydrous ethanol to remove unreacted 3-aminopropyltriethoxysilane, and dry in an oven at 120°C for 2 hours to obtain amino-terminated functionalized magnetic ferroferric oxide nanoparticles (hereinafter referred to as amino-terminated magnetic particles).

[0033] 1 g of the above-mentioned amino magnetic particles was weighed and uniformly dispersed in 100 mL of organic solvent DMF by ultrasound, and then 0.5 g of tetradecyl dicarboxylic acid and 0.05 g of catalyst 4-dimethylaminopyridine were added under mechanical stirring, and the mixture was reacted at 120° C. for 24 hours. The solid product collected by the magnet was washed with anhydrous ethanol and dried in an oven at 120° C. for 2 hours to obtain alkyl carboxylic acid-modified magnetic ferrosoferric oxide nanoparticles.

[0034] Example 4

[0035] Weigh 3.89 g of ferric chloride and 3.34 g of ferrous sulfate heptahydrate and dissolve them in 400 mL of deionized water. Start stirring and heat to 50° C. at 300 rpm. Add 30 mL of 15% sodium hydroxide solution under nitrogen protection. After the addition, continue crystallization for 1 hour. Separate the solid product by a magnet and dry it in an oven at 120° C. for 2 hours to obtain magnetic ferrosoferric oxide nanoparticles.

[0036] Weigh 2 g of the above-mentioned magnetic ferroferric oxide nanoparticles, uniformly disperse them in 200 mL of ethanol by ultrasound, then add 1 g of 3-aminopropyltriethoxysilane under mechanical stirring, react at 30°C for 12 hours, separate the solid product with a magnet, wash with anhydrous ethanol to remove unreacted 3-aminopropyltriethoxysilane, and dry in an oven at 120°C for 2 hours to obtain amino-terminated functionalized magnetic ferroferric oxide nanoparticles (hereinafter referred to as amino-terminated magnetic particles).

[0037] 1 g of the above-mentioned amino magnetic particles was weighed and uniformly dispersed in 100 mL of organic solvent DMF by ultrasound, and then 0.5 g of hexadecyl dicarboxylic acid and 0.05 g of catalyst 4-dimethylaminopyridine were added under mechanical stirring, and the mixture was reacted at 120° C. for 24 hours. The solid product collected by the magnet was washed with anhydrous ethanol and dried in an oven at 120° C. for 2 hours to obtain alkyl carboxylic acid-modified magnetic ferrosoferric oxide nanoparticles.

[0038] Example 5

[0039] Weigh 3.89 g of ferric chloride and 3.34 g of ferrous sulfate heptahydrate and dissolve them in 400 mL of deionized water. Start stirring and heat to 50° C. at 300 rpm. Add 30 mL of 15% sodium hydroxide solution under nitrogen protection. After the addition, continue crystallization for 1 hour. Separate the solid product by a magnet and dry it in an oven at 120° C. for 2 hours to obtain magnetic ferrosoferric oxide nanoparticles.

[0040] Weigh 2 g of the above-mentioned magnetic ferroferric oxide nanoparticles, uniformly disperse them in 200 mL of ethanol by ultrasound, then add 1 g of 3-aminopropyltriethoxysilane under mechanical stirring, react at 30°C for 12 hours, separate the solid product with a magnet, wash with anhydrous ethanol to remove unreacted 3-aminopropyltriethoxysilane, and dry in an oven at 120°C for 2 hours to obtain amino-terminated functionalized magnetic ferroferric oxide nanoparticles (hereinafter referred to as amino-terminated magnetic particles).

[0041] 1 g of the above-mentioned amino magnetic particles was weighed and uniformly dispersed in 100 mL of organic solvent DMF by ultrasound, and then 0.5 g of octadecyl dicarboxylic acid and 0.05 g of catalyst 4-dimethylaminopyridine were added under mechanical stirring, and the mixture was reacted at 120° C. for 24 hours. The solid product collected by the magnet was washed with anhydrous ethanol and dried in an oven at 120° C. for 2 hours to obtain alkyl carboxylic acid-modified magnetic ferrosoferric oxide nanoparticles.

[0042] Application Example 1

[0043] The comparative example of this application implementation uses three kinds of fluorine-containing muds to be filtered as raw materials, and uses the alkyl carboxylic acid modified magnetic ferroferric oxide nanoparticles of Examples 1-5 as filter aids to perform a filtration and dehydration test on the fluorine-containing sludge. The specific steps are as follows: weigh 0.1-0.5g of filter aid and add it to 100g of fluorine-containing mud, stir at room temperature and 300rpm for 5 minutes, then filter with a Buchner funnel with a diameter of 9cm, and the vacuum degree is 0.09MPa. Filter until no liquid drips within 1 minute, record the filtration time and the mass of the wet filter cake, and then put the filter cake into a 120-degree oven to dry to constant weight and record the weight of the dry filter cake, and calculate the moisture content of the wet filter cake. As a blank application example, the above operation is performed without adding any filter aid. It can be seen from Table 1 that compared with the blank test, the filter aids of all examples can shorten the filtration time, and the moisture content of the corresponding wet filter cake is significantly reduced. In addition, among the filter aids of all examples, the filter aid of Example 4 exhibits the best filtration performance.

[0044] Table 1 Effect of filter aid types on filtration and dewatering performance of fluorine-containing mud

[0045]

[0046]

[0047] Application Example 2

[0048] For application test 7 in application example 1, a reuse test of the filter aid was conducted, and the relevant filtration steps were the same as those described in application example 1. A magnet was used to separate the dried fluorine-containing sludge and the filter aid, and the recovered mass of the filter aid was recorded. The mass of the filter aid was slightly lost, mainly due to adhesion to the vessel wall and filter paper during the filtration process. The recovered filter aid was used to conduct the same application test, and was recycled 3 times according to the above method. The corresponding effects are shown in Table 2. The filter aid prepared in the example still maintains excellent filter dehydration performance during the three repeated uses.

[0049] Table 2 Filtration results of using the filter aid of test 7 in Example 1 three times

[0050] Number of times of reuse Filter aid recovery amount / g Filter aid dosage / g Filter time / s Wet cake moisture content / % 1 0.43 0.43 1126 44.52 2 0.38 0.38 1245 45.64 3 0.32 0.32 1317 46.73

[0051] The present invention and its embodiments are described above, but such description is not restrictive. The application example is only one of the embodiments of the present invention, and the actual application mode is not limited thereto. In short, if ordinary technicians in this field are inspired by it, without departing from the purpose of the invention, they can creatively design filter aids and embodiments similar to the technical solution, which should all fall within the protection scope of the present invention.

Claims

1. A reusable filter aid for filtration and dehydration of fluoride-containing sludge, characterized in that: The main component is magnetic ferroferric oxide nanoparticles modified by alkyl carboxylic acid.

2. A method for preparing a reusable filter aid for filtration and dehydration of fluorine-containing sludge as claimed in claim 1, characterized in that: It includes steps (1) to (3): (1) Preparation of magnetic FeO4 nanoparticles by coprecipitation method Weigh 3.89 g of ferric chloride and 3.34 g of ferrous sulfate heptahydrate and dissolve them in 400 mL of deionized water. Start stirring, heat to 50°C at 300 rpm, and drop 30 mL of 15% sodium hydroxide solution under nitrogen protection. After the dropwise addition, continue crystallization for 1 hour. Separate the solid product by a magnet and dry it in an oven at 120°C for 12 hours to obtain magnetic ferrosoferric oxide nanoparticles. (2) Surface amino modification of magnetic FeO nanoparticles Weigh 2 g of the magnetic ferroferric oxide nanoparticles prepared in step (1), and evenly disperse them in 200 mL of ethanol by ultrasonication. Then, add 3-aminopropyltriethoxysilane under mechanical stirring, react at 30° C. for 12 hours, separate the solid product with a magnet, wash with ethanol, and dry in an oven at 120° C. for 12 hours to obtain amino-functionalized magnetic ferroferric oxide nanoparticles (hereinafter referred to as amino-functionalized magnetic particles). (3) Alkyl carboxylic acid modification of magnetic FeO nanoparticles Weigh 1 g of the amino magnetic particles obtained in step (2), and disperse them uniformly in 100 mL of an organic solvent by ultrasonication. Then, add alkyl dicarboxylic acid and a catalyst under mechanical stirring, and react at 120° C. for 24 hours. Collect the solid product by a magnet, wash with anhydrous ethanol, and dry in an oven at 120° C. for 12 hours to obtain alkyl carboxylic acid-modified magnetic ferrosoferric oxide nanoparticles.

3. The method for preparing a reusable filter aid for filtration and dehydration of fluorine-containing sludge according to claim 2, characterized in that: The usage of the 3-aminopropyltriethoxysilane is 0.5 g to 1 g.

4. The method for preparing a reusable filter aid for filtration and dehydration of fluorine-containing sludge according to claim 2, characterized in that: The organic solvent is any one of dimethylformamide (DMF), dimethylacetamide and dimethyl sulfoxide.

5. The method for preparing a reusable filter aid for filtration and dehydration of fluorine-containing sludge according to claim 2, characterized in that: The alkyl dicarboxylic acid is any one of alkyl dicarboxylic acids having different carbon chain lengths, specifically any one of sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid and octadecanedioic acid.

6. The method for preparing a reusable filter aid for filtration and dehydration of fluorine-containing sludge according to claim 2, characterized in that: The usage of the alkyl dicarboxylic acid is 0.2 g to 1 g.

7. The method for preparing a reusable filter aid for filtration and dehydration of fluorine-containing sludge according to claim 2, characterized in that: The catalyst is 4-dimethylaminopyridine, and the usage amount thereof is 0.02g-0.1g.

Citation Information

Patent Citations

  • Environmental-friendly filter aid for aluminium hydroxide dehydration

    CN101664670A

  • Preparation method of anionic ferroferric oxide nano-particles with carboxyl groups on surfaces

    CN105366735A

  • Multi-organic modified magnetic compound and preparation method thereof and application in wastewater treatment

    CN107303483A

  • Kieselguhr composite filter aid preparation method

    CN109019749A

  • Preparation of noble metal magnetic nano-catalyst based on polymerization ionic liquid loading

    CN111068779A

Cited By

  • A chemical filter aid for promoting solid-liquid separation of fluoride-containing sludge and its application method

    CN123105955A