Sanzan glue-based adsorbent as well as preparation method and application thereof

By combining Sanzan glue with other components and adopting specific treatment methods, it solves the problems of poor water resistance and insufficient stability, and prepares a high-efficiency adsorbent, which realizes effective adsorption of heavy metals and dyes in the water body and improves water quality Purification effect.

CN119034690APending Publication Date: 2024-11-29TIANJIN AGRICULTURE COLLEGE
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411390317.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing natural polymer materials such as Sanzan Gummy have problems such as poor water resistance, insufficient stability and weak mechanical strength in water treatment, which limits its application.

Method used

By combining Sanzan gum with components such as bentonite, kaolin and iron oxide, a composite gel ball is formed using a specific preparation method, and treated with inorganic acid or calcium chloride solution to enhance its stability and mechanical strength, a This kind of adsorbent has good water resistance and high efficiency adsorption performance.

Benefits of technology

It improves the water resistance and mechanical strength of the adsorbent, can efficiently adsorb heavy metal ions and cationic dyes in the water body, improves the water quality purification effect, and is simple in preparation, environmentally friendly and non-toxic.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034690A_ABST
    Figure CN119034690A_ABST
Patent Text Reader

Abstract

The invention discloses an adsorbent based on Sanzan gum and a preparation method and application thereof, and belongs to the technical field of adsorbent preparation and water treatment. The preparation method comprises the following steps: carrying out alkali treatment on Sanzan gum, compounding with bentonite, kaolin and iron oxide, preparing composite gel balls based on Sanzan gum by taking inorganic acid or / and calcium chloride as a stationary liquid, and freeze-drying or drying to obtain the Sanzan gum-based adsorbent. The preparation process of the adsorbent is simple and convenient, the adopted raw materials are environment-friendly, toxic organic solvents are not used, and the safety and environment friendliness of the preparation process are ensured; the prepared adsorbent has good mechanical strength and stability, and can efficiently adsorb heavy metal ions and cationic dyes in a water body, so that the water quality purification effect is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adsorbent preparation and water treatment, and specifically is an adsorbent based on trisammonium gum and a preparation method and application thereof. Technical Background

[0002] With the rapid development of modern industry, the resulting environmental pollution problem has become increasingly prominent, especially the pollution of natural water bodies, which has become a public health and safety issue that needs to be solved urgently. Contaminated wastewater contains a large amount of heavy metals and dyes. These pollutants have irreversible and persistent toxicity, posing a serious threat to human health; pollutants in polluted water bodies can enter the human body through the enrichment of the food chain, causing serious damage to the kidneys, liver and brain nerves. In order to effectively remove these pollutants, people have developed a variety of treatment methods, including chemical precipitation, ion exchange, adsorption and membrane filtration. Among these methods, adsorption shows great application potential due to its low cost, high efficiency and environmental friendliness. However, existing adsorption materials, such as sodium alginate and chitosan, still have problems such as insufficient stability, poor water resistance and weak mechanical strength. At present, the development of new adsorption materials has made significant progress, for example: a green and environmentally friendly heavy metal adsorbent based on sodium alginate, a preparation method and application thereof (CN117797776), which discloses a heavy metal adsorbent with sodium alginate, carboxymethyl chitosan, sodium bentonite and polyethylene glycol as a matrix, cross-linked with calcium chloride and modified with 2-morpholineethanesulfonic acid, N-hydroxysuccinimide and 1-ethyl-(3-dimethylaminopropyl)carbodiimide, which can produce a strong adsorption effect on copper ions and lead ions. However, its process is complicated and a large amount of organic reagents are used in the preparation process, which causes potential harm to the environment.

[0003] Sanxan gum is a natural polymer synthesized by fermentation of the bacterium Sphingomonas sanxanigenens. It has the advantages of being safe, non-toxic, completely degradable and renewable. There are a large number of active groups such as hydroxyl and carboxyl groups in its structure, which can provide adsorption sites to remove heavy metals and cationic dyes from water. However, Sanxan gum has problems such as poor water resistance, insufficient stability and weak mechanical strength, which limit its application. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of natural polymer materials such as insufficient stability, poor water resistance and weak mechanical strength, and to provide an adsorbent based on trisammonium gum and a preparation method and application thereof.

[0005] The technical solution adopted by the present invention to solve its technical problem is:

[0006] An adsorbent based on trisammonium gum, and a preparation method and application thereof.

[0007] The adsorbent based on tri-zan gum, its preparation method and application, contains the following ingredients and weight proportions: 0.6-0.8 parts of tri-zan gum, 0-10 parts of bentonite, 0-15 parts of kaolin and 0-1.2 parts of iron oxide.

[0008] The preparation method of the adsorbent based on Sanzan gum as described above comprises the following steps:

[0009] An adsorbent based on trisaccharide gum and a preparation method and application thereof, the method comprising the following steps:

[0010] Step (1): weigh trimethoprim, add water to prepare a trimethoprim solution with a mass volume percentage of 0.6-0.8% under stirring, and continue stirring until it is completely dissolved; add 0-0.01% of alkali with a mass volume percentage, stir at 35-45° C. for 0.5-2h to obtain a trimethoprim solution;

[0011] Step (2): adding bentonite, kaolin and iron oxide to the solution obtained in step (1) according to the above-mentioned component ratios, and stirring and mixing them uniformly;

[0012] Step (3): dripping the solution of step (2) dropwise into a 0.05-0.5M inorganic acid solution, or a 0.5-0.8M calcium chloride solution, or a solution containing both 0.1-0.3M inorganic acid and 0.1-0.2M calcium chloride, and stirring for 5-60 minutes to obtain a composite gel sphere based on trisaccharide;

[0013] Step (4): Filter out the composite gel balls of step (3), rinse with tap water, and freeze-dry in vacuum or dry at 70-80° C. to obtain a tri-zan gum-based adsorbent for use in the adsorption of heavy metals and cationic dyes.

[0014] Furthermore, the adsorbent based on Tri-Gel is characterized in that the molecular marker of Tri-Gel is SEQ ID NO.1 or SEQ ID NO.2.

[0015] Furthermore, the adsorbent based on tribasic gum is characterized in that the iron oxide is ferroferric oxide or ferrous oxide.

[0016] Furthermore, the base in step (1) is sodium hydroxide or potassium hydroxide.

[0017] Furthermore, the inorganic acid in step (3) comprises: hydrochloric acid, boric acid, phosphoric acid or a mixture of two thereof.

[0018] Furthermore, the heavy metals in step (4) include: one or more of copper ions, cadmium ions, manganese ions, lead ions, nickel ions, magnesium ions, and cobalt ions; and the cationic dyes include one or more of methylene blue, crystal violet, and malachite green.

[0019] The use of the tri-zan gum-based adsorbent prepared by the preparation method described above in removing heavy metals and cationic dyes from water bodies.

[0020] The advantages and positive effects achieved by the present invention are:

[0021] The tri-zan gum used in the present invention is a natural polymer synthesized by microorganisms, which has the advantages of being safe, non-toxic, completely degradable, and renewable, and is a green and environmentally friendly adsorption material. The preparation process of the adsorbent is simple, and no toxic organic reagents are used in the preparation process, which ensures the safety and environmental protection of the preparation process. The prepared tri-zan gum-based adsorbent has good water resistance, mechanical strength and stability, and can efficiently adsorb heavy metal ions and cationic dyes in water bodies, thereby improving the water purification effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a scanning electron microscope image of the adsorbent of the present invention, wherein Figure 1 A is the electron microscope image of Example 2, Figure 1 B is the electron microscope image of Example 3, Figure 1 C is the electron microscope image of Example 13, Figure 1 D is the electron microscope image of Example 15.

[0023] Figure 2 This is the adsorption curve of copper ions by the adsorbent in Example 5 of the present invention under different pH conditions.

[0024] Figure 3 This is the adsorption curve of methylene blue by the adsorbent in Example 5 of the present invention under different pH conditions.

[0025] Figure 4 This is a diagram showing the adsorption effect of the magnetic adsorbent on methylene blue in Example 16 of the present invention. DETAILED DESCRIPTION

[0026] The present invention will be further described below in conjunction with the embodiments. The following embodiments are descriptive rather than restrictive, and the protection scope of the present invention cannot be limited by the following embodiments.

[0027] The various experimental operations involved in the specific embodiments are all routine techniques in the art. For parts not specially annotated in this document, ordinary technicians in the art can implement them by referring to various commonly used reference books, scientific and technological literature or related instructions, manuals, etc. before the filing date of this invention.

[0028] Embodiment 1:

[0029] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.6 part of tri-zan gum and 1 part of ferrosoferric oxide.

[0030] The preparation method is as follows:

[0031] Step (1): weigh Tri-gluconate, add water under stirring to prepare a Tri-gluconate solution with a mass volume percentage of 0.6%, and continue stirring until it is completely dissolved to obtain a Tri-gluconate solution.

[0032] Step (2): adding ferrosoferric oxide to the solution obtained in step (1) according to the above-mentioned component ratio, and stirring to mix evenly;

[0033] Step (3): drip the solution of step (2) into 0.05M hydrochloric acid solution drop by drop, stir and fix for 5 minutes, and obtain composite gel spheres based on trisaccharide gel;

[0034] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and vacuum freeze-dry to obtain a triazan gum-based adsorbent.

[0035] Copper nitrate was used to prepare wastewater with a copper ion concentration of 400 mg / L and a pH of 5. The adsorbent was added to the wastewater at a dosage of 5 g / L. The adsorption was carried out on a shaker at 25°C and 100 r / min for 12 hours. The adsorption of copper ions was 5.1 mg / g. Wastewater with a methylene blue concentration of 500 mg / L and a pH of 9 was prepared. The adsorbent was added to the wastewater at a dosage of 2.5 g / L. The adsorption was carried out on a shaker at 25°C and 100 r / min for 4 hours. The adsorption of methylene blue was 172.3 mg / g. However, the adsorbent was partially dissolved after 24 hours, indicating that its water resistance was poor.

[0036] Embodiment 2:

[0037] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.7 parts of tri-zan gum and 10 parts of kaolin.

[0038] The preparation method is as follows:

[0039] Step (1): weigh Tri-glucoside, add water under stirring to prepare a Tri-glucoside solution with a mass volume percentage of 0.7%, and continue stirring until it is completely dissolved to obtain a Tri-glucoside solution;

[0040] Step (2): adding kaolin to the solution obtained in step (1) according to the above-mentioned component ratio, and stirring and mixing uniformly;

[0041] Step (3): drip the solution of step (2) dropwise into a 0.3 M boric acid solution, and stir for 5 min to obtain a composite gel sphere based on trisaccharide gel;

[0042] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and dry at 70° C. to obtain a tris-based adsorbent.

[0043] The hardness of the adsorbent is 2.9 kg, and the SEM structure of the adsorbent is as follows: Figure 1 As shown in A. The adsorbent was added to the wastewater with a copper ion concentration of 400mg / L and pH 5 according to the dosage of 5g / L, and the adsorption was carried out on a shaking table at 25°C and 100r / min for 12h, and the adsorption amount of copper ions was 13.4mg / g. The adsorbent was added to the wastewater with a methylene blue concentration of 500mg / L and pH 9 according to the dosage of 2.5g / L, and the adsorption was carried out on a shaking table at 25°C and 100r / min for 4h, and the adsorption amount of methylene blue was 148.7mg / g, and the appearance of the adsorbent was stable and unchanged after 24h. Compared with Example 1, the adsorbent prepared by drying has lower cost, is suitable for large-scale preparation, and has improved adsorption capacity for copper ions.

[0044] Embodiment 3:

[0045] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.7 parts of tri-zan gum and 5 parts of bentonite.

[0046] The preparation method is as follows:

[0047] Step (1): weigh Tri-glucoside, add water under stirring to prepare a Tri-glucoside solution with a mass volume percentage of 0.7%, and continue stirring until it is completely dissolved to obtain a Tri-glucoside solution;

[0048] Step (2): adding bentonite to the solution obtained in step (1) according to the above-mentioned component ratio, and stirring and mixing uniformly;

[0049] Step (3): drip the solution of step (2) into 0.5 M phosphoric acid solution drop by drop, stir and fix for 5 minutes, and obtain composite gel spheres based on trisaccharide gel;

[0050] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and dry at 80° C. to obtain a tris-based adsorbent.

[0051] The hardness of the adsorbent is 15.1 kg, and the SEM structure of the adsorbent is as follows: Figure 1As shown in B. The adsorbent was added to the wastewater with a copper ion concentration of 400mg / L and pH 5 at a dosage of 5g / L, and adsorbed on a shaking table at 25°C and 100r / min for 12h, and the adsorption amount of copper ions was 12.8mg / g. The adsorbent was added to the wastewater with a methylene blue concentration of 500mg / L and pH 9 at a dosage of 2.5g / L, and adsorbed on a shaking table at 25°C and 100r / min for 4h, and the adsorption amount of methylene blue was 117.5mg / g, and the appearance of the adsorbent was stable and unchanged after 24h. Compared with Example 2, the adsorbent has a higher hardness, is not easily deformed and broken during transportation and use, and can better maintain the integrity of the particle morphology, but the adsorption capacity of copper ions and methylene blue is reduced.

[0052] Embodiment 4:

[0053] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.6 parts of tri-zan gum and 1 part of ferrosoferric oxide.

[0054] The preparation method is as follows:

[0055] Step (1): weigh trimethoprim gum, add water to prepare a trimethoprim gum solution with a mass volume percentage of 0.6% under stirring conditions, and continue stirring until it is completely dissolved; add 0.005% mass volume percentage of potassium hydroxide, stir at 35° C. for 0.5 h, and obtain a trimethoprim gum solution;

[0056] Step (2): adding ferrosoferric oxide to the solution obtained in step (1) according to the above-mentioned component ratio, and stirring to mix evenly;

[0057] Step (3): drip the solution of step (2) into 0.6M calcium chloride solution drop by drop, stir and fix for 30 minutes, to obtain composite gel spheres based on trisaccharide;

[0058] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and vacuum freeze-dry to obtain a triazan gum-based adsorbent.

[0059] The adsorbent was added to wastewater with a copper ion concentration of 400 mg / L and pH 5 at a dosage of 5 g / L, and adsorbed on a shaking table at 25°C and 100 r / min for 12 hours, and the adsorption of copper ions was 77.7 mg / g. The adsorbent was added to wastewater with a methylene blue concentration of 500 mg / L and pH 9 at a dosage of 2.5 g / L, and adsorbed on a shaking table at 25°C and 100 r / min for 4 hours, and the adsorption of methylene blue was 161.6 mg / g, and the appearance of the adsorbent was stable and unchanged after 24 hours. Compared with Example 1, the adsorption capacity of the adsorbent for copper ions is improved.

[0060] Embodiment 5:

[0061] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.6 part of tri-zan gum and 1 part of ferrosoferric oxide.

[0062] The preparation method is as follows:

[0063] Step (1): weigh trimethoprim gum, add water to prepare a trimethoprim gum solution with a mass volume percentage of 0.6% under stirring conditions, and continue stirring until it is completely dissolved; add 0.003% potassium hydroxide with a mass volume percentage, and stir at 35° C. for 0.5 h to obtain a trimethoprim gum solution;

[0064] Step (2): adding ferrosoferric oxide to the solution obtained in step (1) according to the above-mentioned component ratio, and stirring to mix evenly;

[0065] Step (3): dripping the solution of step (2) dropwise into a solution containing 0.1 M hydrochloric acid and 0.2 M calcium chloride, stirring for 15 min, to obtain composite gel spheres based on trisaccharide;

[0066] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and vacuum freeze-dry to obtain a triazan gum-based adsorbent.

[0067] The adsorbent was added to wastewater with a copper ion concentration of 400 mg / L and a pH of 5 at a dosage of 5 g / L. The adsorption was carried out on a shaking table at 25°C and 100 r / min for 12 h. The adsorption amount of copper ions was 119.2 mg / g. The pH of the copper ion-containing wastewater was adjusted to 1 to 5. The adsorption curve under the same conditions is as follows: Figure 2 As shown, the adsorption amount is the highest at pH 5. The adsorbent was added to the wastewater with a methylene blue concentration of 500 mg / L and a pH of 9 at a dosage of 2.5 g / L, and adsorbed on a shaking table at 25°C and 100 r / min for 4 hours. The adsorption amount of methylene blue was 187.1 mg / g. The pH of the above methylene blue-containing wastewater was adjusted to 3 to 12. The adsorption curve under the same conditions is shown in Figure 3 As shown, the adsorption amount is the highest at pH 11, which is 217.1 mg / g, and the appearance of the adsorbent is stable and unchanged after being placed in wastewater under different pH conditions for 48 hours. Compared with Example 1 and Example 4, the adsorbent has improved adsorption capacity for copper ions and methylene blue.

[0068] Embodiment 6:

[0069] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.7 parts of tri-zan gum and 5 parts of kaolin.

[0070] The preparation method is as follows:

[0071] Step (1): weigh trimethoprim, add water to prepare a trimethoprim solution with a mass volume percentage of 0.7% under stirring, and continue stirring until it is completely dissolved; add 0.005% mass volume percentage of sodium hydroxide, stir at 45° C. for 1 hour to obtain a trimethoprim solution;

[0072] Step (2): adding kaolin to the solution obtained in step (1) according to the above-mentioned component ratio, and stirring and mixing uniformly;

[0073] Step (3): drip the solution of step (2) into a 0.6M calcium chloride solution drop by drop, and stir for 60 minutes to obtain a composite gel sphere based on trisaccharide;

[0074] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and dry at 70° C. to obtain a tris-based adsorbent.

[0075] The hardness of the adsorbent is 4.7kg. The adsorbent was added to wastewater with a copper ion concentration of 400mg / L and a pH of 5 at a dosage of 5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 12h. The adsorption of copper ions was 118.8mg / g. The adsorbent was added to wastewater with a methylene blue concentration of 500mg / L and a pH of 9 at a dosage of 2.5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 4h. The adsorption of methylene blue was 211.4mg / g, and the appearance of the adsorbent was stable and unchanged after 24h.

[0076] Embodiment 7:

[0077] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.8 parts of tri-zan gum and 10 parts of kaolin.

[0078] The preparation method is as follows:

[0079] Step (1): weigh trimethoprim, add water to prepare a trimethoprim solution with a mass volume percentage of 0.8% under stirring, and continue stirring until it is completely dissolved; add 0.007% mass volume percentage of sodium hydroxide, stir at 45° C. for 1 hour to obtain a trimethoprim solution;

[0080] Step (2): adding kaolin to the solution obtained in step (1) according to the above-mentioned component ratio, and stirring and mixing uniformly;

[0081] Step (3): drip the solution of step (2) into a 0.6M calcium chloride solution drop by drop, and stir for 60 minutes to obtain a composite gel sphere based on trisaccharide;

[0082] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and dry at 70° C. to obtain a tris-based adsorbent.

[0083] The hardness of the adsorbent is 3.2kg. The adsorbent was added to wastewater with a copper ion concentration of 400mg / L and a pH of 5 at a dosage of 5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 12h. The adsorption of copper ions was 129.9mg / g. The adsorbent was added to wastewater with a methylene blue concentration of 500mg / L and a pH of 9 at a dosage of 2.5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 4h. The adsorption of methylene blue was 258.7mg / g, and the appearance of the adsorbent was stable and unchanged after 24h.

[0084] Embodiment 8:

[0085] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.8 parts of tri-zan gum and 15 parts of kaolin.

[0086] The preparation method is as follows:

[0087] Step (1): weigh trimethoprim, add water to prepare a trimethoprim solution with a mass volume percentage of 0.8% under stirring, and continue stirring until it is completely dissolved; add 0.01% mass volume percentage of sodium hydroxide, stir at 45° C. for 0.5 h, and obtain a trimethoprim solution;

[0088] Step (2): adding kaolin to the solution obtained in step (1) according to the above-mentioned component ratio, and stirring and mixing uniformly;

[0089] Step (3): drip the solution of step (2) into a 0.8M calcium chloride solution drop by drop, and stir for 30 minutes to obtain a composite gel sphere based on trisaccharide;

[0090] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and dry at 70° C. to obtain a tris-based adsorbent.

[0091] The hardness of the adsorbent is 1.6kg. The adsorbent was added to wastewater with a copper ion concentration of 400mg / L and a pH of 5 at a dosage of 5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 12h. The adsorption of copper ions was 107.6mg / g. The adsorbent was added to wastewater with a methylene blue concentration of 500mg / L and a pH of 9 at a dosage of 2.5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 4h. The adsorption of methylene blue was 235.2mg / g, and the appearance of the adsorbent was stable and unchanged after 24h.

[0092] Embodiment 9:

[0093] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.7 parts of tri-zan gum and 10 parts of kaolin.

[0094] The preparation method is as follows:

[0095] Step (1): weigh trimethoprim, add water to prepare a trimethoprim solution with a mass volume percentage of 0.7% under stirring, and continue stirring until it is completely dissolved; add 0.003% mass volume percentage of sodium hydroxide, stir at 45° C. for 1.5 hours to obtain a trimethoprim solution;

[0096] Step (2): adding kaolin to the solution obtained in step (1) according to the above-mentioned component ratio, and stirring and mixing uniformly;

[0097] Step (3): dripping the solution of step (2) dropwise into a solution containing 0.2 M hydrochloric acid and 0.1 M calcium chloride, stirring for 15 min, to obtain composite gel spheres based on trisaccharide;

[0098] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and dry at 70° C. to obtain a tris-based adsorbent.

[0099] The hardness of the adsorbent is 4.1kg. The adsorbent was added to wastewater with a copper ion concentration of 400mg / L and a pH of 5 at a dosage of 5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 12h. The adsorption of copper ions was 138.4mg / g. The adsorbent was added to wastewater with a methylene blue concentration of 500mg / L and a pH of 9 at a dosage of 2.5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 4h. The adsorption of methylene blue was 309.8mg / g, and the appearance of the adsorbent was stable and unchanged after 48h.

[0100] Embodiment 10:

[0101] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.7 parts of tri-zan gum, 13 parts of kaolin, and 1 part of ferrosoferric oxide.

[0102] The preparation method is as follows:

[0103] Step (1): weigh trimethoprim, add water to prepare a trimethoprim solution with a mass volume percentage of 0.7% under stirring, and continue stirring until it is completely dissolved; add 0.005% mass volume percentage of sodium hydroxide, stir at 45° C. for 1 hour to obtain a trimethoprim solution;

[0104] Step (2): adding kaolin and ferroferric oxide to the solution obtained in step (1) according to the above-mentioned component ratio, and stirring and mixing uniformly;

[0105] Step (3): dripping the solution of step (2) dropwise into a solution containing 0.3 M hydrochloric acid and 0.1 M calcium chloride, stirring for 60 min, to obtain composite gel spheres based on trisaccharide;

[0106] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and dry at 70° C. to obtain a tris-based adsorbent.

[0107] The hardness of the adsorbent is 3.9kg. The adsorbent was added to wastewater with a copper ion concentration of 400mg / L and a pH of 5 at a dosage of 5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 12h. The adsorption of copper ions was 102.1mg / g. The adsorbent was added to wastewater with a methylene blue concentration of 500mg / L and a pH of 9 at a dosage of 2.5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 4h. The adsorption of methylene blue was 265.6mg / g, and the appearance of the adsorbent was stable and unchanged after 48h.

[0108] Embodiment 11:

[0109] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.7 parts of tri-zan gum, 10 parts of kaolin, and 1.2 parts of ferric oxide.

[0110] The preparation method is as follows:

[0111] Step (1): weigh trimethoprim, add water to prepare a trimethoprim solution with a mass volume percentage of 0.7% under stirring, and continue stirring until it is completely dissolved; add 0.005% mass volume percentage of sodium hydroxide, stir at 45° C. for 1 hour to obtain a trimethoprim solution;

[0112] Step (2): adding kaolin and ferric oxide to the solution obtained in step (1) according to the above-mentioned component ratio, and stirring and mixing evenly;

[0113] Step (3): dripping the solution of step (2) dropwise into a solution containing 0.3 M phosphoric acid and 0.2 M calcium chloride, stirring for 60 min, to obtain composite gel spheres based on trisaccharide;

[0114] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and dry at 70° C. to obtain a tris-based adsorbent.

[0115] The hardness of the adsorbent is 3.0kg. The adsorbent was added to wastewater with a copper ion concentration of 400mg / L and a pH of 5 at a dosage of 5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 12h. The adsorption of copper ions was 133.1mg / g. The adsorbent was added to wastewater with a methylene blue concentration of 500mg / L and a pH of 9 at a dosage of 2.5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 4h. The adsorption of methylene blue was 272.4mg / g, and the appearance of the adsorbent was stable and unchanged after 48h.

[0116] Embodiment 12:

[0117] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.7 parts of tri-zan gum and 2 parts of bentonite.

[0118] The preparation method is as follows:

[0119] Step (1): weigh trimethoprim, add water to prepare a trimethoprim solution with a mass volume percentage of 0.7% under stirring, and continue stirring until it is completely dissolved; add 0-0.005% potassium hydroxide with a mass volume percentage, stir at 35° C. for 2 hours to obtain a trimethoprim solution;

[0120] Step (2): adding bentonite to the solution obtained in step (1) according to the above-mentioned component ratio, and stirring and mixing uniformly;

[0121] Step (3): drip the solution of step (2) dropwise into a 0.5 M calcium chloride solution, and stir for 60 min to obtain a composite gel sphere based on trisaccharide;

[0122] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and dry at 80° C. to obtain a tris-based adsorbent.

[0123] The hardness of the adsorbent is 13.4kg. The adsorbent was added to wastewater with a copper ion concentration of 400mg / L and a pH of 5 at a dosage of 5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 12h. The adsorption of copper ions was 117.7mg / g. The adsorbent was added to wastewater with a methylene blue concentration of 500mg / L and a pH of 9 at a dosage of 2.5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 4h. The adsorption of methylene blue was 139.3mg / g, and the appearance of the adsorbent was stable and unchanged after 24h.

[0124] Embodiment 13:

[0125] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.7 parts of tri-zan gum and 5 parts of bentonite.

[0126] The preparation method is as follows:

[0127] Step (1): weigh trimethoprim, add water to prepare a trimethoprim solution with a mass volume percentage of 0.7% under stirring, and continue stirring until it is completely dissolved; add 0-0.005% potassium hydroxide with a mass volume percentage, stir at 35° C. for 2 hours to obtain a trimethoprim solution;

[0128] Step (2): adding bentonite to the solution obtained in step (1) according to the above-mentioned component ratio, and stirring and mixing uniformly;

[0129] Step (3): drip the solution of step (2) dropwise into a 0.5 M calcium chloride solution, and stir for 60 min to obtain a composite gel sphere based on trisaccharide;

[0130] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and dry at 80° C. to obtain a tris-based adsorbent.

[0131] The hardness of the adsorbent is 10.3 kg, and the SEM structure of the adsorbent is as follows: Figure 1 As shown in Figure C, it can be observed that the surface of the adsorbent is rougher and more fluffy, and the larger specific surface area of ​​the adsorbent provides more adsorption sites. The adsorbent was added to the wastewater with a copper ion concentration of 400 mg / L and a pH of 5 at a dosage of 5 g / L, and adsorbed on a shaking table at 25°C and 100 r / min for 12 hours. The adsorption of copper ions was 146.5 mg / g. The adsorbent was added to the wastewater with a methylene blue concentration of 500 mg / L and a pH of 9 at a dosage of 2.5 g / L, and adsorbed on a shaking table at 25°C and 100 r / min for 4 hours. The adsorption of methylene blue was 149.7 mg / g, and the appearance of the adsorbent was stable and unchanged after 24 hours.

[0132] Embodiment 14:

[0133] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.8 parts of tri-zan gum and 10 parts of bentonite.

[0134] The preparation method is as follows:

[0135] Step (1): weigh trimethoprim, add water to prepare a trimethoprim solution with a mass volume percentage of 0.8% under stirring, and continue stirring until it is completely dissolved; add potassium hydroxide with a mass volume percentage of 0-0.008%, and stir at 35° C. for 2 hours to obtain a trimethoprim solution;

[0136] Step (2): adding bentonite to the solution obtained in step (1) according to the above-mentioned component ratio, and stirring and mixing uniformly;

[0137] Step (3): drip the solution of step (2) dropwise into a 0.7 M calcium chloride solution, and stir for 60 min to obtain a composite gel sphere based on trisaccharide;

[0138] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and dry at 80° C. to obtain a tris-based adsorbent.

[0139] The hardness of the adsorbent is 8.8kg. The adsorbent was added to wastewater with a copper ion concentration of 400mg / L and a pH of 5 at a dosage of 5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 12h. The adsorption of copper ions was 138.9mg / g. The adsorbent was added to wastewater with a methylene blue concentration of 500mg / L and a pH of 9 at a dosage of 2.5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 4h. The adsorption of methylene blue was 156.0mg / g, and the appearance of the adsorbent was stable and unchanged after 24h.

[0140] Embodiment 15:

[0141] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.8 parts of tri-zan gum and 5 parts of bentonite.

[0142] The preparation method is as follows:

[0143] Step (1): weigh trimethoprim, add water to prepare a trimethoprim solution with a mass volume percentage of 0.8% under stirring, and continue stirring until it is completely dissolved; add potassium hydroxide with a mass volume percentage of 0-0.006%, and stir at 35° C. for 1.5 hours to obtain a trimethoprim solution;

[0144] Step (2): adding bentonite to the solution obtained in step (1) according to the above-mentioned component ratio, and stirring and mixing uniformly;

[0145] Step (3): dripping the solution of step (2) dropwise into a solution containing 0.2 M hydrochloric acid and 0.1 M calcium chloride, stirring for 15 min, to obtain composite gel spheres based on trisaccharide;

[0146] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and dry at 80° C. to obtain a tris-based adsorbent.

[0147] The hardness of the adsorbent is 9.6 kg, and the SEM structure of the adsorbent is as follows: Figure 1 As shown in D, more network structures can be observed on the surface of the adsorbent. The adsorbent was added to the wastewater with a copper ion concentration of 400 mg / L and a pH of 5 at a dosage of 5 g / L, and adsorbed on a shaking table at 25°C and 100 r / min for 12 hours. The adsorption of copper ions was 154.0 mg / g. The adsorbent was added to the wastewater with a methylene blue concentration of 500 mg / L and a pH of 9 at a dosage of 2.5 g / L, and adsorbed on a shaking table at 25°C and 100 r / min for 4 hours. The adsorption of methylene blue was 180.3 mg / g, and the appearance of the adsorbent was stable and unchanged after 48 hours.

[0148] Embodiment 16:

[0149] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.8 parts of tri-zan gum, 5 parts of bentonite, and 0.8 parts of ferrosoferric oxide.

[0150] The preparation method is as follows:

[0151] Step (1): weigh trimethoprim, add water to prepare a trimethoprim solution with a mass volume percentage of 0.8% under stirring, and continue stirring until it is completely dissolved; add potassium hydroxide with a mass volume percentage of 0-0.008%, and stir at 35° C. for 2 hours to obtain a trimethoprim solution;

[0152] Step (2): Add bentonite and ferroferric oxide to the solution obtained in step (1) according to the above-mentioned component ratio, and stir to mix evenly;

[0153] Step (3): dripping the solution of step (2) dropwise into a solution containing 0.3 M hydrochloric acid and 0.1 M calcium chloride, stirring for 20 min, to obtain composite gel spheres based on trisaccharide;

[0154] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and dry at 80° C. to obtain a tris-based adsorbent.

[0155] The hardness of the adsorbent is 11.6kg. The adsorbent was added to wastewater with a copper ion concentration of 400mg / L and a pH of 5 at a dosage of 5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 12h. The adsorption of copper ions was 138.3mg / g. The adsorbent was added to wastewater with a methylene blue concentration of 500mg / L and a pH of 9 at a dosage of 2.5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 4h. The adsorption of methylene blue was 169.1mg / g, and the appearance of the adsorbent was stable and unchanged after 48h. The adsorption effect of the magnetic adsorbent on methylene blue is as follows Figure 4 shown.

[0156] Embodiment 17:

[0157] An adsorbent based on tri-zan gum contains the following ingredients and weight proportions: 0.8 parts of tri-zan gum, 7 parts of bentonite, and 1 part of ferric oxide.

[0158] The preparation method is as follows:

[0159] Step (1): weigh trimethoprim, add water to prepare a trimethoprim solution with a mass volume percentage of 0.8% under stirring, and continue stirring until it is completely dissolved; add 0.008% potassium hydroxide with a mass volume percentage, and stir at 35° C. for 2 hours to obtain a trimethoprim solution;

[0160] Step (2): Add bentonite and ferric oxide to the solution obtained in step (1) according to the above-mentioned component ratio, and stir to mix evenly;

[0161] Step (3): dripping the solution of step (2) dropwise into a solution containing 0.3 M hydrochloric acid and 0.15 M calcium chloride, stirring for 30 min, to obtain composite gel spheres based on trisaccharide;

[0162] Step (4): Filter out the composite gel balls from step (3), rinse with tap water, and dry at 80° C. to obtain a tris-based adsorbent.

[0163] The hardness of the adsorbent is 7.9kg. The adsorbent was added to wastewater with a copper ion concentration of 400mg / L and a pH of 5 at a dosage of 5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 12h. The adsorption of copper ions was 149.6mg / g. The adsorbent was added to wastewater with a methylene blue concentration of 500mg / L and a pH of 9 at a dosage of 2.5g / L, and adsorbed on a shaking table at 25℃ and 100r / min for 4h. The adsorption of methylene blue was 150.8mg / g, and the appearance of the adsorbent was stable and unchanged after 24h.

[0164] Embodiment 18:

[0165] Detection method based on adsorbent of trisammonium gum.

[0166] Take the adsorbent based on tri-zan gum in Example 1, grind it, add 9 times the mass of deionized water, vortex mix evenly, let it stand for 8h at 4°C, centrifuge it at 3000r / min for 15min, take the supernatant, use the bacterial genomic DNA extraction kit, extract the genomic DNA according to the instructions, and perform electrophoresis detection. Use the extracted DNA as a template, 5'TAAGGTCCCCAAGTCACGTC3' as the upstream primer, 5'TCTCTCAAGCGCCTTGGTAT 3' as the downstream primer, and perform PCR amplification. The PCR amplification system is: 1μL of 10-30ng / uL template DNA, 0.5μL of 10μM upstream primer and downstream primer, 0.5μL of 10mM dNTP, 2.5μL of 10× buffer, 0.5μL of 5U / μL Taq enzyme, and add ultrapure water to 25μL. The PCR reaction conditions were: 95°C pre-denaturation for 5 min; 94°C for 45 s, 59°C for 45 s, 72°C for 1 min, 30 cycles; 72°C extension for 10 min. The PCR amplification band detected by electrophoresis was about 560 bp. The PCR amplification product was sequenced by DNA, and the sequences near the primers that affected the sequencing accuracy were removed to obtain the specific molecular marker SEQ ID NO.1 representing Trisammonium.

[0167]

[0168]

[0169] Embodiment 19:

[0170] Detection method based on adsorbent of trisammonium gum.

[0171] Take the adsorbent based on tri-zan gum in Example 15, grind it, add 9 times the mass of deionized water, vortex mix evenly, let it stand for 8h at 4°C, centrifuge it at 3000r / min for 15min, take the supernatant, use the bacterial genomic DNA extraction kit, extract the genomic DNA according to the instructions, and perform electrophoresis detection. Use the extracted DNA as a template, 5'TCAGGCCGTGTGGGGAA3' as the upstream primer, and 5'GATCCGATCCAGCTTTCGGG 3' as the downstream primer to perform PCR amplification. The PCR amplification system is: 1μL of 10-30ng / uL template DNA, 0.5μL of 10μM upstream primer and downstream primer, 10mM dNTP 1.0μL, 10× buffer 2.5μL, 5U / μL Platinum Taq DNA polymerase 0.5μL, add ultrapure water to 25μL. The PCR reaction conditions were: 95°C pre-denaturation for 5 min; 94°C for 45 s, 62°C for 45 s, 72°C for 1 min, 30 cycles; 72°C extension for 10 min. The PCR amplification band detected by electrophoresis was about 950 bp. The PCR amplification product was sequenced by DNA, and the sequences near the primers that affected the sequencing accuracy were removed to obtain the specific molecular marker SEQ ID NO.2 representing Trisammonium.

[0172]

[0173] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.

Claims

1. An adsorbent based on trisaccharide gum, characterized in that: Its components and weight proportions are as follows: 0.6-0.8 parts of Sanzan gum, 0-10 parts of bentonite, 0-15 parts of kaolin, and 0-1.2 parts of iron oxide; The preparation method of the adsorbent based on Sanzan gum as described above comprises the following steps: Step (1): weigh trimethoprim, add water to prepare a trimethoprim solution with a mass volume percentage of 0.6-0.8% under stirring, and continue stirring until it is completely dissolved; add 0-0.01% of alkali with a mass volume percentage, stir at 35-45° C. for 0.5-2h to obtain a trimethoprim solution; Step (2): adding bentonite, kaolin and iron oxide to the solution obtained in step (1) according to the above-mentioned component ratios, and stirring and mixing them uniformly; Step (3): dripping the solution of step (2) dropwise into a 0.05-0.5M inorganic acid solution, or a 0.5-0.8M calcium chloride solution, or a solution containing both 0.1-0.3M inorganic acid and 0.1-0.2M calcium chloride, and stirring for 5-60 minutes to obtain a composite gel sphere based on trisaccharide; Step (4): Filter out the composite gel balls of step (3), rinse with tap water, and freeze-dry in vacuum or dry at 70-80° C. to obtain a tri-zan gum-based adsorbent for use in the adsorption of heavy metals and cationic dyes.

2. The adsorbent based on trisaccharide gum according to claim 1, characterized in that: The molecular marker of the tri-zan gum is SEQ ID NO.1 or SEQ ID NO.

2.

3. The adsorbent based on trisaccharide gum according to claim 1, characterized in that: The iron oxide is ferroferric oxide or ferrous oxide.

4. The preparation method according to claim 1, characterized in that: The alkali in step (1) is sodium hydroxide or potassium hydroxide; The inorganic acid in step (3) includes: hydrochloric acid, boric acid, phosphoric acid or a mixture of two thereof; the heavy metal in step (4) includes: one or more of copper ion, cadmium ion, manganese ion, lead ion, nickel ion, magnesium ion and cobalt ion; the cationic dye includes one or more of methylene blue, crystal violet and malachite green.

5. Use of the adsorbent based on trisaccharide prepared by the preparation method according to any one of claims 1 to 4 in removing heavy metals and cationic dyes from water.

Citation Information

Patent Citations

  • Green and environment-friendly heavy metal adsorbent based on sodium alginate as well as preparation method and application thereof

    CN117797776A