Titanium dioxide microsphere-based composite particle, preparation method and application

By covering precious metal nanoparticles on titanium dioxide microspheres, titanium dioxide microsphere-based composite particles were prepared, and ultraviolet photocatalytic degradation of electroplating additive JGB was used to solve the problems of low degradation efficiency and complex preparation in the prior art, and efficient JGB degradation was achieved Effect.

CN119034726APending Publication Date: 2024-11-29UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411138806.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently degrade the electroplating additive JGB, especially in the preparation of photocatalysts, which require high-pressure equipment and are not degradable in high degradation efficiency.

Method used

Precious metal nanoparticles were used to cover spherical anatase titanium dioxide microspheres, and titanium dioxide microsphere-based composite particles were prepared by annealing and electroless plating, and photocatalytic degradation was performed by ultraviolet light irradiation.

Benefits of technology

It improves the degradation efficiency of JGB by about 30%, and has a simple process, precise control of the material composition and structure, avoids the agglomeration of composite particles, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034726A_ABST
    Figure CN119034726A_ABST
Patent Text Reader

Abstract

The invention provides a titanium dioxide microsphere-based composite particle as well as a preparation method and application thereof, and belongs to the technical field of photocatalytic degradation. The composite particles are obtained by covering spherical anatase type titanium dioxide with noble metal nanoparticles. After two hours of ultraviolet irradiation, the degradation effect of the composite particles on JGB can be improved by about 30% compared with the degradation effect of only titanium dioxide microspheres on JGB.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photocatalytic degradation, and specifically relates to titanium dioxide microsphere-based composite particles, a preparation method and an application thereof. Background Art

[0002] Electroplating plays an irreplaceable role in industry, and various wastes are inevitably generated during the electroplating process, especially the electroplating additive JGB. The electroplating additive JGB is widely used in the electroplating process, especially in processes such as black nickel plating and zinc plating, to improve the appearance and performance of the coating. However, this additive and its waste are potentially harmful to the environment. The JGB additive components contained in electroplating wastewater will enter the water body, causing water pollution. Its organic compounds are difficult to biodegrade and may have toxic effects on aquatic organisms, destroying the aquatic ecosystem.

[0003] To improve this problem, existing technologies have been used for treatment, including biodegradation, physical adsorption, incineration and photocatalytic degradation. Among these technologies, photocatalytic degradation technology has attracted much attention due to its high degradation efficiency and broad spectrum. At the same time, it also has the advantages of low energy consumption, simple process and warm reaction conditions. The efficiency of photocatalytic reaction is determined by the catalytic activity of the photocatalyst. At present, photocatalysts mainly include transition metals (zinc-based, titanium-based, iron-based) and aluminum-based oxides, which use external energy to generate electron-hole pairs to achieve catalytic degradation. Among them, titanium dioxide-based catalysts are non-toxic and harmless materials, do not produce secondary pollution during the reaction, and are environmentally friendly; they have good chemical stability and physical stability, and can still maintain efficient catalytic performance after repeated use. They have been widely used in the photodegradation of organic pollutants. However, the band gap of TiO2 is 3.2eV, which is a wide band gap semiconductor, and high-energy ultraviolet (UV) is required to generate electron-hole pairs.

[0004] In order to overcome the above problems, the prior art improves the photocatalytic activity of titanium dioxide-based catalysts by combining the surface plasmon resonance (SPR) effect. Olaniyan Ibukun's document (Olaniyan Ibukun, Jeong Hae-Kyung. Tailo ring titanium dioxide by silver particles for photocatalysis [J]. Current Applied Physics, 2020, 20 (1): 23-28.) discloses a catalyst of precious metal nanoparticles plus TiO2 for photocatalytic degradation. However, the hydrothermal method is used to synthesize TiO2-Ag composite materials in the document, which requires the use of high-voltage equipment, is complex to operate, has high safety requirements and is not suitable for synthesizing materials that require large-scale production. At the same time, this additive is only used to achieve the degradation of methyl blue (MB), and the degradation efficiency is not high enough.

[0005] Therefore, how to prepare titanium dioxide-based catalysts so that they can efficiently degrade JGB has become a research focus. Summary of the invention

[0006] In view of the problems existing in the background technology, the purpose of the present invention is to provide a titanium dioxide microsphere-based composite particle, a preparation method and an application. The composite particle is obtained by covering spherical anatase titanium dioxide with precious metal nanoparticles, and the particle has an excellent degradation effect on Janus green dye.

[0007] To achieve the above object, the technical solution of the present invention is as follows:

[0008] A titanium dioxide microsphere-based composite particle, wherein the composite particle is obtained by covering spherical anatase titanium dioxide with noble metal nanoparticles; the diameter of the spherical anatase titanium dioxide is 500nm-900nm, the particle size of the noble metal nanoparticles is 40nm-100nm; the coverage rate of the noble metal nanoparticles on the spherical anatase titanium dioxide is 30%-50%.

[0009] Furthermore, the noble metal nanoparticles are gold nanoparticles or silver nanoparticles.

[0010] A method for preparing titanium dioxide microsphere-based composite particles comprises the following steps:

[0011] Step 1: synthesizing amorphous titanium dioxide microspheres with uniform particle size and smooth surface;

[0012] Step 2: Convert the amorphous titanium dioxide microspheres obtained in step 1 into anatase titanium dioxide. The specific process is as follows:

[0013] The amorphous titanium dioxide microspheres are placed in a muffle furnace for annealing to transform the amorphous titanium dioxide into anatase titanium dioxide;

[0014] Step 3: The anatase titanium dioxide obtained in step 2 is sensitized with a tin sensitizing solution, and then noble metal particles are deposited on the surface of the titanium dioxide by a reduction method to obtain the desired titanium dioxide microsphere-based composite particles.

[0015] Furthermore, the specific process of step 1 is:

[0016] Step 1.1. Preparation of precursor solution: dissolve tetrabutyl titanate in ethylene glycol. The solution is milky white. Stir until the solution becomes colorless to obtain a precursor solution.

[0017] Step 1.2. Under stirring conditions, add the precursor solution to the organic solvent, then add the stabilizer, and finally slowly add deionized water. Stop stirring when the solution turns milky white again;

[0018] Step 1.3. The reaction solution of step 1.2 is allowed to stand for a while. After the reaction is complete, the milky white solution is centrifuged and the precipitate is washed to obtain amorphous titanium dioxide microspheres.

[0019] Furthermore, in step 2, the annealing temperature is 300° C.-500° C., and the annealing time is 3 h-6 h.

[0020] Furthermore, in step 3, the tin sensitizing solution includes methanol, water, SnCl2 and trifluoroacetic acid.

[0021] The present invention also provides the use of the titanium dioxide microsphere-based composite particles in photocatalytic degradation, specifically: adding the titanium dioxide microsphere-based composite particles into a certain concentration of Janus Green dye, and then irradiating with ultraviolet light to perform photodegradation.

[0022] Furthermore, the specific parameters of the ultraviolet lamp irradiation are: ultraviolet power is 80W-120W, and wavelength is 200nm-300nm.

[0023] The mechanism of the present invention is as follows: the present invention combines a layer of precious metal nanoparticles on the titanium dioxide spherical shell by chemical plating on the surface of anatase titanium dioxide, and the uniform spherical structure can plate the precious metal particles more stably, and the specific coverage rate can gather energy more concentratedly, thereby improving the degradation ability. At the same time, spherical anatase titanium dioxide with a diameter of 500nm-900nm is specifically selected, and the titanium dioxide microspheres within this diameter range can efficiently focus energy on the silver nanoparticles and have an anti-agglomeration effect, thereby avoiding direct agglomeration of the composite particles in the electroplating solution salt solution rich in JGB, thereby having an excellent degradation effect on JGB.

[0024] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0025] The composite material photocatalytic particles are obtained by using silver particles loaded on the surface of micron-sized titanium dioxide microspheres, which can be used for the photodegradation of dyes in electroplating solutions. After two hours of ultraviolet light irradiation, the degradation effect of the composite particles of the present invention on JGB can be improved by about 30% compared with the degradation effect of only titanium dioxide microspheres on JGB. This is because compared with pure anatase titanium dioxide, the nanocomposite material of silver-doped titanium dioxide can reduce the band gap between the valence band and the conduction band, expand the light absorption range of TiO2, reduce the recombination rate of electrons and holes, and increase the redox reaction time, so that it has a better degradation effect. At the same time, the present invention uses a sol-gel method to synthesize the TiO2-Ag composite material, which can accurately control the composition and structure of the material, and the process is relatively simple, and the prepared photocatalytic particles do not agglomerate. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a scanning electron microscope image of the titanium dioxide microsphere-based composite particles of the present invention.

[0027] Figure 2 This is a scanning electron microscope image of anatase titanium dioxide.

[0028] Figure 3 Device diagram for the photocatalytic degradation process.

[0029] Figure 4 This is an ultraviolet spectrum diagram of the photocatalytic degradation of JGB by titanium dioxide microsphere-based composite particles and titanium dioxide microspheres alone in Example 1 of the present invention.

[0030] Figure 5 This is an ultraviolet spectrum diagram of the photocatalytic degradation of JGB by titanium dioxide microsphere-based composite particles and titanium dioxide microspheres alone in Example 2 of the present invention.

[0031] Figure 6 It is the ultraviolet spectrum of the photocatalytic degradation of JGB by titanium dioxide microsphere-based composite particles and titanium dioxide microspheres alone in the comparative example of the present invention. DETAILED DESCRIPTION

[0032] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with the implementation modes and the accompanying drawings.

[0033] A titanium dioxide microsphere-based composite particle, the scanning electron microscope image of the composite particle is as follows Figure 1 As shown in FIG. 1 , the precious metal nanoparticles are coated on the spherical anatase titanium dioxide; wherein the scanning electron microscope image of the anatase titanium dioxide is as shown in FIG. Figure 2 As shown, the anatase titanium dioxide is spherical and evenly distributed without clusters, and its diameter is 500nm-900nm; the noble metal nanoparticles are gold nanoparticles or silver nanoparticles, and their particle size is 40nm-100nm; the coverage of the noble metal nanoparticles is 30%-50%.

[0034] Example 1

[0035] A method for preparing titanium dioxide microsphere-based composite particles comprises the following steps:

[0036] Step 1: Synthesize titanium dioxide microspheres with uniform particle size and smooth surface; Specific process:

[0037] Step 1.1. Preparation of precursor solution: 0.23 g of tetrabutyl titanate was dissolved in 50 g of ethylene glycol (0.45 w / w). The solution was milky white. After stirring for 8 hours, the solution became colorless to obtain a precursor solution.

[0038] Step 1.2. Under stirring, add 15 ml of the precursor solution to 60 ml of acetone, then add 60 μl of stabilizer glacial acetic acid, and finally slowly add 300 μl of water. Stir for 1 hour until the solution turns milky white. Let it stand for one day until the reaction is complete.

[0039] Step 1.3. The milky white solution obtained in step 1.2 is centrifuged, and the precipitate is washed twice with deionized water and once with ethanol to obtain titanium dioxide microspheres, and then the titanium dioxide microspheres are dispersed in deionized water for storage to obtain a titanium dioxide microsphere solution;

[0040] Step 2: Prepare spherical anatase titanium dioxide, the specific process is:

[0041] Step 2.1. Centrifuge the titanium dioxide solution obtained in step 1, discard the supernatant, wash the lower white solid and dry it in a vacuum drying oven at 80°C;

[0042] Step 2.2. The dried titanium dioxide microsphere powder is placed in a muffle furnace for annealing at a temperature of 400°C for 3 hours to obtain anatase titanium dioxide;

[0043] Step 3: Depositing precious metal particles on the surface of anatase titanium dioxide. Specific process:

[0044] Step 3.1. First, sensitize the anatase titanium dioxide: clean the 3 cm 2 The titanium dioxide is immersed in 27 ml of tin sensitization solution, and the mixture is gently shaken for sensitization for 30 minutes; then the obtained sample is fully washed to remove the chloride ions in the system, and the sensitized anatase titanium dioxide is obtained;

[0045] The tin sensitization solution includes 13.5 mL of methanol, 13.5 mL of water, 0.20 g of SnCl2, and 225 μL of trifluoroacetic acid;

[0046] Step 3.2. Depositing silver nanoparticles on the surface of the sensitized anatase titanium dioxide, with a coverage rate of 35% of the silver nanoparticles: immersing the sensitized anatase titanium dioxide in 27 ml of silver ammonia solution, placing it in a dark environment for 5 minutes, then adding 9 ml of the glucose mixed solution, and continuing to react in a dark environment for 30 minutes, silver nanoparticles can be generated on the surface of the anatase titanium dioxide;

[0047] The preparation process of the silver ammonia solution is as follows: 50 ml of 0.003 mol / L KOH solution is added to 10 ml of 0.03 mol / L concentrated silver nitrate solution, the solution changes from transparent to light yellow, and then ammonia water is added dropwise to the solution until it becomes transparent; the glucose mixed solution is prepared from 0.23 g of sodium citrate, 0.16 g of glucose and 9 ml of water.

[0048] The titanium dioxide microsphere-based composite particles prepared in this embodiment are used to photocatalytically degrade JGB. The specific process is as follows:

[0049] 0.006 g of titanium dioxide microsphere-based composite particles were added to 10 ppm of electroplating additives (mainly JGB), ultrasonically dispersed, and placed in a glass sample bottle; the glass sample bottle was then placed in a rotating disk of a photocatalytic degradation device, as shown in the schematic diagram of the device structure. Figure 3 As shown, it includes a darkroom, an ultraviolet lamp and a rotating disk; wherein the ultraviolet lamp is fixedly set in the center of the darkroom, and the rotating disk is placed vertically and its height is parallel to the ultraviolet lamp. During photodegradation, the rotating disk rotates under the irradiation of the ultraviolet lamp, driving the adsorption-desorption balance between the organic dye and the photocatalyst, so that the titanium dioxide microsphere composite particles are better mixed in the JGB; the ultraviolet lamp power is 100W and the wavelength is 254nm.

[0050] The ultraviolet spectrum of the photocatalytic degradation of this embodiment is as follows Figure 4 As shown in the figure, the red line is the degradation curve of JGB by anatase titanium dioxide microspheres only, and the blue curve is the degradation curve of JGB by titanium dioxide microsphere-based composite particles prepared in this embodiment; it can be seen from the figure that after two hours of ultraviolet light irradiation, only anatase titanium dioxide microspheres and titanium dioxide microsphere-based composite particles have degradation effects on JGB, degrading 76% and 86% respectively, indicating that the titanium dioxide microsphere-based composite particles prepared by the present invention can effectively improve the degradation effect and have excellent degradation efficiency.

[0051] Example 2

[0052] Titanium dioxide microsphere-based composite particles were prepared according to the method of Example 1, except that the time for depositing silver nanoparticles in step 3.2 was adjusted to adjust the coverage of the silver nanoparticles to 42%, and the other steps remained unchanged.

[0053] The ultraviolet spectrum of photocatalytic degradation in this embodiment is as follows Figure 5 As shown in the figure, only the anatase titanium dioxide microspheres and titanium dioxide microsphere-based composite particles degraded 76% and 98% of JGB respectively after two hours of UV irradiation; the performance was improved by about 30%.

[0054] Comparative Example 1

[0055] Titanium dioxide microsphere-based composite particles were prepared according to the method of Example 1, except that the time for depositing silver nanoparticles in step 3.2 was adjusted to adjust the coverage of the silver nanoparticles to 10%, and the other steps remained unchanged.

[0056] The ultraviolet spectrum of photocatalytic degradation in this embodiment is as follows Figure 6 As shown in the figure, only the anatase titanium dioxide microspheres and titanium dioxide microsphere-based composite particles degraded 76% and 80% of JGB respectively after two hours of UV irradiation, indicating that when the coverage is low, the contribution to the degradation performance does not meet the requirements.

[0057] The above description is only a specific implementation mode of the present invention. Any feature disclosed in this specification, unless otherwise stated, can be replaced by other alternative features that are equivalent or have similar purposes; all the disclosed features, or all the steps in the methods or processes, except for mutually exclusive features and / or steps, can be combined in any way.

Claims

1. A titanium dioxide microsphere-based composite particle, characterized in that: The composite particles are obtained by covering spherical anatase titanium dioxide with precious metal nanoparticles; the diameter of the spherical anatase titanium dioxide is 500nm-900nm, the particle size of the precious metal nanoparticles is 40nm-100nm; the coverage rate of the precious metal nanoparticles on the spherical anatase titanium dioxide is 30%-50%.

2. The titanium dioxide microsphere-based composite particles according to claim 1, characterized in that: The noble metal nanoparticles are gold nanoparticles or silver nanoparticles.

3. A method for preparing titanium dioxide microsphere-based composite particles, characterized in that: The following steps are involved: Step 1: synthesizing amorphous titanium dioxide microspheres with uniform particle size and smooth surface; Step 2: Convert the amorphous titanium dioxide microspheres obtained in step 1 into anatase titanium dioxide. The specific process is as follows: The amorphous titanium dioxide microspheres are placed in a muffle furnace for annealing to transform the amorphous titanium dioxide into anatase titanium dioxide; Step 3: The anatase titanium dioxide obtained in step 2 is sensitized with a tin sensitizing solution, and then noble metal particles are deposited on the surface of the titanium dioxide by a reduction method to obtain the desired titanium dioxide microsphere-based composite particles.

4. The preparation method according to claim 3, characterized in that: The specific process of step 1 is: Step 1.

1. Preparation of precursor solution: dissolve tetrabutyl titanate in ethylene glycol. The solution is milky white. Stir until the solution becomes colorless to obtain a precursor solution. Step 1.

2. Under stirring conditions, add the precursor solution to the organic solvent, then add the stabilizer, and finally slowly add deionized water. Stop stirring when the solution turns milky white again; Step 1.

3. The reaction solution of step 1.2 is allowed to stand for a while. After the reaction is complete, the milky white solution is centrifuged and the precipitate is washed to obtain amorphous titanium dioxide microspheres.

5. The preparation method according to claim 3, characterized in that: In step 2, the annealing temperature is 300° C.-500° C., and the annealing time is 3 h-6 h.

6. The preparation method according to claim 3, characterized in that: In step 3, the tin sensitizing solution includes methanol, water, SnCl2 and trifluoroacetic acid.

7. An application of titanium dioxide microsphere-based composite particles prepared by the preparation method according to any one of claims 3 to 6 in photocatalytic degradation, characterized in that: Specifically, titanium dioxide microsphere-based composite particles are added into a certain concentration of Janus Green dye, and then irradiated with ultraviolet light for photodegradation.

8. The use according to claim 7, characterized in that The specific parameters of ultraviolet lamp irradiation are: ultraviolet power is 80W-120W, and wavelength is 200nm-300nm.

Citation Information

Cited By

  • Titanium dioxide / gold composite material as well as preparation method and application thereof