Thin film type TiO2 / (MoP / CdS) composite photocatalyst as well as preparation and application thereof

Through the preparation of thin-film TiO2/(MoP/CdS) composite photocatalyst, the problems of low visible light utilization efficiency and low photogenerated carrier separation efficiency in photocatalytic hydrogen production technology are solved, and efficient photocatalytic decomposition of water is achieved. It has good stability and low cost characteristics.

CN119034771APending Publication Date: 2024-11-29NINGXIA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411142729.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing photocatalytic hydrogen production technology faces the problems of low visible light utilization efficiency, low photocarrier separation efficiency and high cost, which leads to the general limitation of the conversion efficiency of solar hydrogen production.

Method used

The film-type TiO2/(MoP/CdS) composite photocatalyst is used to prepare TiO2/(MoP/CdS) powder photocatalyst by hydrothermal calcining method, and bond it to plexiglass to form a film, and fixed it with adhesive. Increase the rate of hydrogen production by photocatalytic decomposition of water.

Benefits of technology

The rate of hydrogen production by photocatalytic decomposition of water is significantly improved. The photocatalytic hydrogen production activity of powdered TiO2/(MoP/CdS) is 33.4 times that of single CdS, the stability of the film type reaches 150 hours, and the process is simple and the raw material cost is low.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034771A_ABST
    Figure CN119034771A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and an application method of a film type TiO2 / (MoP / CdS) composite photocatalyst. The preparation method comprises the following steps: firstly, preparing a powder TiO2 / (MoP / CdS) composite catalyst by a hydrothermal-calcination method, and then loading the powder catalyst on a polymethyl methacrylate (PMMA) organic glass plate by using an adhesive to form a thin film type structure with the thickness of about 12.3 microns. The film type TiO2 / (MoP / CdS) composite photocatalyst shows excellent catalytic performance and stability, has the advantages of simple preparation process, relatively low raw material cost and the like, and is suitable for expanded-area photocatalytic hydrogen production application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thin film TiO 2 Preparation and application of MoP / CdS composite photocatalyst. The composite photocatalyst is used for photocatalytic decomposition of water to produce hydrogen, showing a high rate of photocatalytic decomposition of water to produce hydrogen, and is also expected to be applied in other fields. Background Art

[0002] The excessive consumption of fossil fuels not only leads to the release of a large amount of carbon dioxide, exacerbating environmental pollution and the greenhouse effect, but also faces the serious problem of resource depletion. In order to meet this challenge, photocatalytic water splitting to produce hydrogen as a promising green technology has attracted widespread attention and exploration.

[0003] The main challenges faced by photocatalytic hydrogen production are closely related to several factors. First, the utilization efficiency of visible light is limited, which directly affects the efficiency of photocatalytic hydrogen production. In addition, the low efficiency and high cost of photogenerated carrier separation associated with co-catalysts limit the overall efficiency and practical application of the hydrogen production process. The use of different forms of catalysts (such as powders or films) in the reaction system also increases the complexity and limitations of the process. These challenges together lead to the current general limitations on the efficiency of solar hydrogen conversion. Summary of the invention

[0004] The purpose of the present invention is to combine MoP with TiO 2 , and CdS catalysts to increase the rate of hydrogen production from photocatalytic water decomposition.

[0005] Technical solution of the present invention

[0006] A thin film TiO 2 / (MoP / CdS) composite photocatalyst, characterized in that it comprises a substrate and a TiO 2 / (MoP / CdS) powder photocatalyst,

[0007] MoP is 1.8%-11.8% (preferably 5%-7%) of the mass of MoP / CdS (Wt%);

[0008] TiO 2 TiO 2 / (MoP / CdS) mass (Wt%) is 10.0%-50.0% (preferably 25.0%-50.0%).

[0009] TiO 2 The MoP / CdS powder photocatalyst is fixed on the surface of the substrate by adhesive to form a layer of TiO 2 / (MoP / CdS) powder photocatalyst thin film layer.

[0010] The substrate is a flat plate of polymethyl methacrylate (PMMA) organic glass, and the adhesive is covered on one side of the organic glass to form an adhesive layer. 2 / (MoP / CdS) powder is evenly spread on the surface of the adhesive layer and fixed to one surface of the organic glass through the adhesive layer.

[0011] The adhesive includes one or more of acrylic acid water-based adhesive, acrylate adhesive, or double-sided adhesive;

[0012] The thickness of the adhesive layer is 100-200μm, 25cm 2 TiO attached to the substrate surface 2 The amount of MoP / CdS powder photocatalyst is 4-14.2 mg (preferably 8-10 mg).

[0013] The specific preparation process is as follows: take an area of ​​25cm 2 Clean one side of the surface of the polymethyl methacrylate (PMMA) organic glass and evenly cover it with adhesive (with a thickness of 100-200 μm) to form an adhesive layer on the cleaned side;

[0014] Weigh 4-14.2 mg (preferably 8-10 mg) TiO 2 / (MoP / CdS) powder is evenly spread on the surface of the adhesive layer.

[0015] TiO 2 The TiO / (MoP / CdS) composite photocatalyst was prepared by hydrothermal-calcination method using titanium dioxide, molybdenum phosphide and cadmium nitrate as raw materials. 2 / (MoP / CdS) powder photocatalyst;

[0016] 1) The specific process of preparing MoP / CdS is as follows: first, according to the mass ratio (Wt%) of MoP to MoP / CdS being 1.8%-11.8% (preferably 5%-7%), weigh the required amount of MoP and CdS, 0.2-0.4g in total, and add them to 20-40mL of absolute ethanol; then, perform ultrasonic treatment for 0.5-2 hours (preferably 0.5-1 hour); stir the above solution, evaporate to dryness, grind, and finally obtain a solid MoP / CdS composite catalyst (particle size range 40-200nm);

[0017] 2) TiO 2 The specific process of the TiO / (MoP / CdS) catalyst is as follows: First, 2 TiO 2 The mass ratio (Wt%) of TiO / (MoP / CdS) is 10.0%-50.0% (preferably 25.0%-50.0%), and the required amount of TiO2 and MoP / CdS 0.2-0.4 g; the weighed MoP / CdS was added to 30-60 mL of ethanol and treated under ultrasonication for 2-3 hours to form a suspension A; then, the weighed TiO 2 , and similarly perform ultrasonic treatment for 2-3 hours to form suspension B; add suspension B to suspension A and stir to mix the two evenly; then transfer the mixed solution to a hydrothermal reactor and perform hydrothermal reaction at 110-130°C for 1-4 hours; after the reaction, wash with deionized water and absolute ethanol, and then perform vacuum drying at 60-80°C for 8-24 hours to finally obtain powdered TiO 2 / (MoP / CdS) composite catalyst (particle size range 20-200nm).

[0018] TiO 2 The specific preparation process is as follows: under magnetic stirring, 2.0-2.5mL (preferably 2.06-2.10mL) of tetrabutyl titanate is added to a solution containing 8-12mL (preferably 10mL) of glycerol and 55-60mL (preferably 58-60mL) of ethanol; after stirring for 20-40 minutes, the mixed solution is transferred to a 100mL Teflon-lined autoclave and subjected to a hydrothermal reaction at 160-200°C (preferably 180-185°C) for 24-25 hours. Then, the obtained white powder is collected, washed with absolute ethanol, and dried at 60-80°C (preferably 60-65°C) for 10-12 hours; the white powder is transferred to an alumina crucible and calcined at 400-500°C (preferably 460-480°C) for 1.0-1.2 hours, with a heating rate of 5°C / min -1 To obtain TiO 2 (particle size range 20-60nm);

[0019] The specific preparation process of CdS is as follows: First, prepare 0.28 mol / L cadmium nitrate (Cd(NO 3 ) 2 ·4H 2 O) and 0.28 mol / L sodium sulfide (Na 2 S.9H 2 Subsequently, 30 mL of 0.28 mol / L Na 2 S solution was slowly added dropwise to 25 mL, and 0.28 mol / L Cd(NO 3 ) 2solution; after stirring for 20-40 minutes, the mixed solution is transferred to a 100 mL Teflon-lined autoclave, and a hydrothermal reaction is carried out at 160-200° C. (preferably 180-185° C.) for 24-25 hours; after the reaction is completed, the mixture is centrifuged twice with deionized water and absolute ethanol, and then dried at 60-80° C. (preferably 60-65° C.) for 10-12 hours to obtain CdS (particle size range 40-80 nm);

[0020] The specific preparation process of MoP is as follows: weigh 199.8-200.6 mg MoO 3 (preferably 199.9-200.1 mg) and 3.9-4.1 g NaH 2 PO 2 -H 2 O (preferably 4.0 g) is mixed evenly and then fully ground. Subsequently, the mixture is transferred to an alumina crucible and calcined at 680-720°C (preferably 700-710°C) for 1-2 hours at a heating rate of 2-5°C / min; after cooling, the obtained black solid is immersed in a 1-2 mol / L HCl solution to remove impurities; finally, it is washed four times with deionized water to achieve neutralization, and then dried at 60-90°C (preferably 75-85°C) for 12-14 hours to obtain MoP (particle size range 50-200 nm).

[0021] The TiO prepared by the preparation method 2 / (MoP / CdS) composite photocatalyst.

[0022] The thin film TiO 2 Application of / (MoP / CdS) composite photocatalyst as photocatalyst in photocatalytic water decomposition to produce hydrogen.

[0023] TiO 2 The preparation method of / (MoP / CdS) composite photocatalyst, the specific steps are as follows:

[0024] (1) Preparation of TiO 2 The specific process is as follows: 2.068 mL of tetrabutyl titanate was added to a solution containing 10 mL of glycerol and 58 mL of ethanol under magnetic stirring. After stirring for 30 minutes, the mixed solution was transferred to a 100 mL Teflon-lined autoclave and subjected to a hydrothermal reaction at 180 ° C for 24 hours. Then, the obtained white powder was collected, washed with absolute ethanol, and dried at 60 ° C for 12 hours. The white powder was transferred to an alumina crucible and calcined at 470 ° C for 1 hour with a heating rate of 5 ° C / min to obtain TiO 2 .

[0025] (2) Specific process of preparing CdS: First, prepare 0.28 mol / L cadmium nitrate (Cd(NO3 ) 2 ·4H 2 O) and 0.28 mol / L sodium sulfide (Na 2 S.9H 2 Subsequently, 30 mL of 0.28 mol / L Na 2 S solution was slowly added dropwise to 25 mL, and 0.28 mol / L Cd(NO 3 ) 2 After stirring for 30 minutes, the mixed solution was transferred to a 100 mL Teflon-lined autoclave and subjected to a hydrothermal reaction at 180 °C for 24 hours. After the reaction, it was centrifuged twice with deionized water and absolute ethanol, and then dried at 60 °C for 12 hours to obtain CdS.

[0026] (3) The specific process of preparing MoP is as follows: weigh 200.0 mg MoO 3 and 4.0 g NaH 2 PO 2 -H 2 O was mixed evenly and then ground thoroughly. Subsequently, the mixture was transferred to an alumina crucible and calcined at 700 °C for 1 hour with a heating rate of 5 °C / min. After cooling, the obtained black solid was immersed in a 1 mol / L HCl solution to remove impurities. Finally, it was washed four times with deionized water to achieve neutralization and then dried at 80 °C for 12 hours to obtain MoP.

[0027] (4) The specific process of preparing MoP / CdS is as follows:

[0028] First, according to the mass ratio (Wt%) of MoP and MoP / CdS of 2%, 4%, 6%, 8%, 10%, (preferably 6%), the required amount of MoP and CdS are weighed, 30 mL of absolute ethanol is added, and then ultrasonic treatment is performed for 1 hour. The above solution is stirred, evaporated to dryness, ground, and finally a solid MoP / CdS composite catalyst is obtained.

[0029] (5)TiO 2 The specific preparation process of / (MoP / CdS) composite photocatalyst is as follows:

[0030] According to TiO 2 and TiO 2 The mass ratio (Wt%) of TiO / (MoP / CdS) is 16.7%, 25.0%, 33.3%, 50% (preferably 33.3%). 2 MoP / CdS was added to 45 mL of ethanol and treated under ultrasonication for 2 hours to form suspension A. An appropriate amount of TiO 2Add 15 mL of ethanol and perform ultrasonic treatment for 2 hours to form suspension B. Slowly add suspension B to suspension A while stirring to mix the two evenly. Next, transfer the mixed solution to a 100 mL Teflon-lined hydrothermal reactor and perform hydrothermal reaction at 120 ° C for 2 hours. After the reaction, wash with deionized water and absolute ethanol, and then vacuum dry at 60 ° C overnight to obtain powdered TiO 2 / (MoP / CdS) composite catalyst.

[0031] (6) Thin film TiO 2 The specific preparation process of the TiO / (MoP / CdS) composite photocatalyst is as follows: clean the 5*5cm polymethyl methacrylate (PMMA) organic glass surface with deionized water and ethanol, and evenly cover it with adhesive. Weigh 10 mg of the obtained TiO 2 / (MoP / CdS) powder is evenly spread on the surface.

[0032] TiO 2 / (MoP / CdS) composite photocatalyst is used in the photocatalytic water decomposition reaction to produce hydrogen.

[0033] Test conditions: 90 mL of deionized water, 10 mL of lactic acid, a 300W xenon lamp with full wavelength as the sunlight simulation light source, an operating current of 15 mA, an illumination time of 1 h, and Ar gas as the carrier gas;

[0034] In the above, "adhesive glue" refers to the material used to bond the components of the composite photocatalyst together. Specifically, these adhesive glues include acrylic water-based adhesives (formed by copolymerization of pure acrylic ester monomers), acrylate adhesives (such as polymers of methyl acrylate, ethyl acrylate, 2-methyl methacrylate and 2-ethyl methacrylate), or double-sided adhesives. These adhesive glues can be used alone or in combination to achieve the desired bonding effect;

[0035] Advantages of the present invention: the use of TiO 2 Powder and thin film TiO were prepared by using a catalyst that forms a heterojunction structure with CdS and a non-precious metal compound MoP as a co-catalyst for the photocatalyst. 2 / (MoP / CdS), which has a simple preparation method, abundant reserves and low cost. Through the photocatalytic hydrogen production test, it is known that powdered TiO 2 / (MoP / CdS) photocatalytic hydrogen production activity is 42.2mmol / g / h, which is 33.4 times that of single CdS photocatalytic water decomposition hydrogen production activity. 2 / (MoP / CdS) has a photocatalytic hydrogen production activity of 35.5 mmol / g / h, and its stability reaches 150 hours.

[0036] The thin film TiO 2 / (MoP / CdS) composite photocatalyst exhibits excellent catalytic performance and stability, and has the advantages of simple preparation process and relatively low raw material cost, and is suitable for photocatalytic hydrogen production applications in expanded areas. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 Photocatalytic hydrogen production activity relationship diagram of Example 1;

[0038] Figure 2 Photocatalytic hydrogen production activity relationship diagram of Example 2;

[0039] Figure 3 Example 1 (MoP accounts for 6.02% of the mass of MoP / CdS), 2 (TiO 2 The XRD pattern of the loading amount is 34.2%;

[0040] Figure 4 Example 3 (TiO in thin film photocatalyst 2 / (MoP / CdS) loading is 10 mg) XRD pattern;

[0041] Figure 5 Different TiO 2 / (MoP / CdS) loading amount of thin film photocatalyst for hydrogen production activity;

[0042] Figure 6 Example 3 (TiO in thin film photocatalyst 2 / (MoP / CdS) loading amount 10mg) photocatalytic hydrogen production activity stability diagram;

[0043] Figure 7 Example 3 (TiO in thin film photocatalyst 2 / (MoP / CdS) loading is 10 mg) SEM image;

[0044] Figure 8 10 mg of TiO in powder / film form of Example 4 2 / (MoP / CdS) photocatalyst hydrogen production activity diagram;

[0045] Fig. 9 Relationship diagram of the photocatalytic hydrogen production activity of MoP / CdS in powder / thin film form of Example 5;

[0046] Fig.10 TiO in powder / film form of Example 6 2 / (Mo 2 C / CdS) photocatalytic hydrogen production activity relationship diagram. DETAILED DESCRIPTION

[0047] The present invention is further described in detail below through specific examples.

[0048] The MoP used in the following examples was prepared according to the following process: 200.0 mg MoO 3 and 4.0 g NaH 2 PO 2 -H 2 O was mixed and ground thoroughly. Subsequently, the mixture was transferred to an alumina crucible and calcined at 700 °C for 1 hour, with a heating rate of 5 °C / min from room temperature to the calcination temperature. -1 After cooling, the obtained black solid was immersed in 500 mL of 1 mol / L HCl solution to remove impurities. Finally, it was washed four times with deionized water to achieve neutralization (pH = 7) and then dried at 80 °C for 12 h to obtain MoP with a particle size range of 80-180 nm.

[0049] The TiO 2 All were prepared according to the following process: 2.068 mL of tetrabutyl titanate was added to a solution containing 10 mL of glycerol and 58 mL of ethanol under magnetic stirring. After stirring for 30 minutes, the mixed solution was transferred to a 100 mL Teflon-lined autoclave and subjected to a hydrothermal reaction at 180 °C for 24 hours. Then, the obtained white powder was collected, washed with absolute ethanol, and dried at 60 °C for 12 hours. The white powder was transferred to an alumina crucible and calcined at 470 °C for 1 hour, with a heating rate of 5 °C / min from room temperature to the calcination temperature. -1 To obtain TiO 2 The particle size range is 20-30 nm. The CdS used in the following examples was prepared by the following process: 30 mL of Na 2 S.9H 2 O (0.28 M) aqueous solution was added dropwise to 25 mL Cd(NO 3 ) 2 ·4H 2 O (0.28M) aqueous solution, after adding dropwise, stirring was continued for 30 minutes, and then the above solution was transferred to a hydrothermal kettle and reacted in a 180°C forced air drying oven for 24 hours; cooled to room temperature, centrifuged and washed, and the precipitate was transferred to 60°C and dried for 12 hours, and then ground to obtain a CdS catalyst with a particle size range of 50-60nm.

[0050] The photocatalytic hydrogen production reaction conditions used in the following examples are: a 300W xenon lamp with full light band is used as the sunlight simulation light source, and the irradiation area is 25cm 2, working current is 15mA, illumination time is 1h. The reaction solution is 10% volume concentration lactic acid solution, volume is 100ml.

[0051] Embodiment 1:

[0052] 1) Preparation of MoP / CdS composite photocatalyst:

[0053] First, 5.0 mg, 10.0 mg, 16.0 mg, 21.5 mg and 28.0 mg of MoP were weighed, and then different masses of MoP and 0.25 g of CdS were added to 30 mL of absolute ethanol, and then ultrasonically treated for 1 hour. The above solutions were stirred and evaporated to dryness, ground, and finally solid MoP / CdS composite catalysts (MoP accounted for 1.96%, 3.85%, 6.02%, 7.92%, and 10.07% of the mass of MoP / CdS, respectively) were obtained, and the particle size range was 50-100 nm.

[0054] 2) Photocatalytic hydrogen production reaction: 0.1 g MoP / CdS photocatalyst was added to a mixed solution of lactic acid and deionized water. The volume of the mixed solution was 100 mL, including 90 mL of deionized water solution and 10 mL of lactic acid solution. A 300 W xenon lamp with full wavelength was used as the sunlight simulation light source, and the irradiation area was 25 cm 2 , working current is 15mA, and illumination time is 1h.

[0055] 3) In this reaction, when the loading amount of MoP was 6.02%, the maximum hydrogen production from the photocatalytic decomposition of water by MoP / CdS was 3.43 mmol, which was 24.4 times higher than that of CdS alone (using an equal mass of CdS to replace MoP / CdS, and the rest of the process and conditions were the same as step 2 above).

[0056] Embodiment 2:

[0057] 1) Preparation of TiO 2 / (MoP / CdS) powder type composite photocatalyst:

[0058] 0.25 g of MoP / CdS with a loading of 6.02% prepared in Example 1 was added to 45 mL of ethanol and treated under ultrasonication for 2 hours to form a suspension A. Subsequently, 0.25 g, 0.13 g, 0.08 g, 0.06 g and 0.05 g of TiO 2, and ultrasonic treatment was also performed for 2 hours to form suspension B. Suspension B was slowly added to suspension A, and stirred at the same time to mix the two evenly. Next, the mixed solution was transferred to a 100mL Teflon-lined hydrothermal reactor and subjected to hydrothermal reaction at 120°C for 2 hours. After the reaction, it was washed with deionized water and absolute ethanol in turn, and then vacuum dried at 60°C overnight (12h) to finally obtain powdered TiO 2 / (MoP / CdS) composite catalyst (TiO 2 TiO 2 / (MoP / CdS) mass is 50.0%, 34.2%, 24.2%, 19.4%, 16.7% respectively), and the particle size range is 20-80nm.

[0059] 2) Photocatalytic hydrogen production reaction: 0.1g TiO 2 / (MoP / CdS) photocatalyst was added into a mixed solution of lactic acid and deionized water, the volume of the mixed solution was 100 mL, the deionized water solution was 90 mL, the lactic acid solution was 10 mL, the light source was a 300W xenon lamp with full light band as the sunlight simulation light source, and the irradiation area was 25 cm 2 , working current is 15mA, and illumination time is 1h.

[0060] 3) In this reaction, TiO 2 When the loading amount of TiO is 34.2%, 2 The maximum hydrogen production of (MoP / CdS) photocatalytic water decomposition was 4.22 mmol, which was 33.4 times higher than that of CdS alone (using an equal mass of CdS instead of TiO 2 / (MoP / CdS), the rest of the process and conditions are the same as step 2 above), which is 1.2 times higher than that of MoP / CdS (using the same mass of MoP / CdS instead of TiO 2 / (MoP / CdS), the rest of the process and conditions are the same as step 2).

[0061] Embodiment 3:

[0062] 1) Preparation of TiO 2 / (MoP / CdS) thin film composite photocatalyst:

[0063] The surface of polymethyl methacrylate (PMMA) organic glass with a length*width=5*5cm was cleaned with deionized water and ethanol in turn, and the adhesive layer on one side of the organic glass was evenly covered with the adhesive HK-5081 (double-sided adhesive, width 50mm, length 50m) purchased by Ningxia Juhetai Technology Co., Ltd. (thickness 120-140μm). 5.0mg, 8.0mg, 10.0mg, 11.0mg, 12.0mg and 13.0mg (the maximum coating amount can be 14.2mg, and 40%-95% of the area within this coating amount range is exposed outside the adhesive layer) prepared in Example 2 were weighed. 2 The loading amount of TiO is 34.2% 2 / (MoP / CdS) powder composite catalyst was evenly coated on the surface of Hesdick HK-5081 adhesive (purchased from Ningxia Polytech Technology Co., Ltd., double-sided adhesive) (the loading density was 0.20 mg / cm 2 , 0.32mg / cm 2 , 0.4mg / cm 2 , 0.44mg / cm 2 , 0.48mg / cm 2 , 0.52mg / cm 2 ).

[0064] 2) Photocatalytic hydrogen production reaction: TiO 2 / (MoP / CdS) film was placed in a mixed solution of lactic acid and deionized water. The volume of the mixed solution was 100 mL, including 90 mL of deionized water solution and 10 mL of lactic acid solution. The light source was a 300W xenon lamp with a wavelength of 320 nm to 780 nm as a sunlight simulation light source. The irradiation area was 25 cm 2 , working current is 15mA, and illumination time is 1h.

[0065] 3) Photocatalytic stability test: TiO 2 / (MoP / CdS) film was placed in a mixed solution containing lactic acid and deionized water, with a total volume of 100 mL, of which the deionized water solution was 90 mL and the lactic acid solution was 10 mL. After the air in the reaction system was evacuated for 30 minutes, a 300W xenon lamp with a wavelength range of 320nm to 780nm was used to irradiate the solution for hydrogen production stability test. Each cycle test lasted for 5 hours. After the test, the system was vacuumed to keep the volume of the reaction solution unchanged, and the next cycle was continued. A total of 30 cycles of hydrogen production tests were performed.

[0066] 4) In this reaction, when TiO 2 When the loading amount of / (MoP / CdS) is 10.0 mg, TiO 2 / (MoP / CdS) thin film composite photocatalyst decomposes water to produce hydrogen at a rate of 35.5mmol / h / g. 2 The stability of MoP / CdS thin film composite photocatalyst was studied for 150 hours. Within 50 hours, the thin film catalyst remained basically stable, but the activity decreased. After 50 hours, the hydrogen production rate continued to decrease (from 84.1mmol / g to 23.2mmol / g). Interestingly, after 100 hours, the hydrogen production activity was restored to a level comparable to that at 50 hours (79.0mmol / g) by adding 10 ml of lactic acid to the system. The continuous decrease in hydrogen production is due to the continuous consumption of the hole sacrificial agent (lactic acid). After replenishing lactic acid, the hydrogen production performance was restored. However, the continuous hydrogen production still showed a downward trend. This phenomenon is mainly caused by the uneven exposure of the film surface due to the continuous shedding of hydrogen bubbles on the film surface and the continuous consumption of lactic acid.

[0067] Embodiment 4:

[0068] 1) Preparation of TiO 2 / (MoP / CdS) powder type composite photocatalyst:

[0069] 0.25 g of MoP / CdS with a loading of 6.0% prepared in Example 1 was added to 45 mL of ethanol and treated under ultrasonication for 2 hours to form a suspension A. Subsequently, 0.25 g of TiO 2 , and ultrasonic treatment was also performed for 2 hours to form suspension B. Suspension B was slowly added to suspension A while stirring to mix the two evenly. Next, the mixed solution was transferred to a 100mL Teflon-lined hydrothermal reactor and subjected to hydrothermal reaction at 120°C for 2 hours. After the reaction, it was washed with deionized water and absolute ethanol, and then vacuum dried at 60°C overnight to finally obtain powdered TiO 2 / (MoP / CdS) composite catalyst (TiO 2 TiO 2 / (MoP / CdS) mass 50%), with a particle size range of 20-80nm.

[0070] 2) Preparation of TiO 2 / (MoP / CdS) thin film composite photocatalyst:

[0071] The 5*5cm PMMA organic glass surface was cleaned with deionized water and ethanol, and the surface was evenly covered with Hesdick HK-5081 adhesive (purchased from Ningxia Juhetai Technology Co., Ltd., double-sided adhesive with a width of 50mm and a length of 50m) (thickness of 120-140μm) to form an adhesive layer on one side of the organic glass. Weigh 10.0mg of the obtained TiO 2 / (MoP / CdS) powder is evenly applied on the surface of the adhesive layer (load density is 0.4 mg / cm 2 ) to prepare three identical films 1, 2 and 3 (for parallel experiments).

[0072] 3) Photocatalytic hydrogen production reaction: 10 mg TiO 2 / (MoP / CdS) powder and the TiO prepared in step 2 2 / (MoP / CdS) films were placed in a mixed solution of lactic acid and deionized water, the volume of the mixed solution was 100 mL, the deionized water solution was 90 mL, the lactic acid solution was 10 mL, the light source was a 300W xenon lamp with a wavelength of 320nm-780nm as a sunlight simulation light source, and the irradiation area was 25cm 2 , working current is 15mA, and illumination time is 1h.

[0073] 3) In this reaction system, 10 mg TiO 2 The photocatalytic hydrogen production rate of / (MoP / CdS) powder under stirring conditions was 34.1mmol / h / g, while that under non-stirring conditions was 19.9mmol / h / g. 2 / (MoP / CdS) film has a photocatalytic hydrogen production rate of 41.6, 39.2 and 37.5 mmol / h / g (corresponding to the hydrogen production rates of films 1, 2 and 3, respectively) under non-stirring conditions, which is significantly higher than that of powder-type catalysts. This phenomenon may be attributed to the fact that the powder-type catalyst makes the solution turbid during stirring, thereby reducing the transmittance and causing light shielding between particles, which in turn affects the light absorption efficiency. Relatively speaking, the thin-film photocatalyst effectively avoids the turbidity problem of the reaction solution, ensuring that the light energy is uniform and directly irradiated to the catalyst surface, and thus exhibits higher hydrogen production activity. In addition, the recovery of thin-film catalysts is more convenient and does not require complex processing processes such as centrifugation.

[0074] Embodiment 5:

[0075] 1) Preparation of MoP / CdS powder composite photocatalyst:

[0076] First, 16.0 mg of MoP and 0.25 g of CdS were weighed and added to 30 mL of absolute ethanol, and then ultrasonically treated for 1 hour. The above solution was stirred and evaporated to dryness, and ground to finally obtain a solid MoP / CdS composite catalyst (MoP accounts for 6.02% of the mass of MoP / CdS) with a particle size range of 50-100 nm.

[0077] 2) Preparation of MoP / CdS thin film composite photocatalyst:

[0078] The 5*5cm PMMA organic glass surface was cleaned with deionized water and ethanol, and the surface of one side of the organic glass was evenly covered with Hesdick HK-5081 adhesive (purchased from Ningxia Juhetai Technology Co., Ltd., double-sided adhesive, 50mm wide and 50m long) (thickness 120-140μm) to form an adhesive layer. 10.0mg of the obtained MoP / CdS powder was weighed and evenly applied on the surface of the adhesive layer (load density 0.40mg / cm 2 ) to prepare three identical films 1, 2 and 3 (for parallel experiments).

[0079] 3) Photocatalytic hydrogen production reaction: 10 mg of MoP / CdS powder and the MoP / CdS film prepared in step 2 were placed in a mixed solution of lactic acid and deionized water, respectively. The volume of the mixed solution was 100 mL, including 90 mL of deionized water solution and 10 mL of lactic acid solution. A 300 W xenon lamp with a wavelength of 320 nm to 780 nm was used as a sunlight simulation light source, and the irradiation area was 25 cm 2 , working current is 15mA, and illumination time is 1h.

[0080] 3) In this reaction, the photocatalytic decomposition of water by 10 mg MoP / CdS powder under stirring conditions produces hydrogen at a rate of 19.1 mmol / h / g, while the photocatalytic decomposition of water by 10 mg MoP / CdS powder under non-stirring conditions produces hydrogen at a rate of 14.2 mmol / h / g. The photocatalytic decomposition of water by MoP / CdS thin films under non-stirring conditions produces hydrogen at rates of 39.4, 32.0, and 28.8 mmol / h / g (corresponding to the hydrogen production rates of thin films 1, 2, and 3, respectively), all showing more efficient hydrogen production activity than the powder type. The photocatalytic reaction process of powder photocatalysts requires constant stirring to improve the uniform absorption of light by the catalyst under illumination. Continuous mechanical stirring is very energy-consuming. In addition, powder catalysts are not conducive to separation from the reaction solution, and therefore, powder photocatalysts are considered to be unfavorable for large-scale hydrogen production. In contrast, preparing photocatalysts for water decomposition in the form of thin films rather than powders has many advantages in terms of improved light absorption efficiency, flexible recyclability, improved anti-precipitation stability, and better size control.

[0081] Embodiment 6:

[0082] 1) Preparation of TiO 2 / (Mo 2 C / CdS) powder type composite photocatalyst:

[0083] First, weigh 55.0 mg of Mo 2 C and 0.25 g CdS were added to 30 mL of absolute ethanol and then ultrasonicated for 1 hour. The above solution was stirred and evaporated to dryness, ground, and finally solid Mo was obtained. 2 C / CdS composite catalyst (Mo 2 C accounts for Mo 2 C / CdS mass 18.02%), particle size range 50-100nm. 2 C / CdS was added to 45 mL of ethanol and treated under ultrasonication for 2 h to form suspension A. Subsequently, 0.25 g of TiO 2 , and ultrasonic treatment was also performed for 2 hours to form suspension B. Suspension B was slowly added to suspension A, and stirred at the same time to mix the two evenly. Next, the mixed solution was transferred to a 100mL Teflon-lined hydrothermal reactor and subjected to hydrothermal reaction at 120°C for 2 hours. After the reaction, it was washed with deionized water and absolute ethanol in turn, and then vacuum dried at 60°C overnight (12h) to finally obtain powdered TiO 2 / (Mo 2 C / CdS) composite catalyst (TiO 2 TiO 2 / (Mo 2 C / CdS) by mass).

[0084] 2) Preparation of TiO 2 / (Mo 2 C / CdS) thin film composite photocatalyst:

[0085] The 5*5cm PMMA organic glass surface was cleaned with deionized water and ethanol, and the surface of one side of the organic glass was evenly covered with Hesdick HK-5081 adhesive (purchased from Ningxia Juhetai Technology Co., Ltd., double-sided adhesive, 50mm wide and 50m long) (thickness 120-140μm) to form an adhesive layer. 10.0mg of the obtained TiO 2 / (Mo 2 C / CdS) powder is evenly applied on the surface of the adhesive layer (load density is 0.40 mg / cm 2 ) to prepare three identical films 1, 2 and 3 (for parallel experiments).

[0086] 3) Photocatalytic hydrogen production reaction: 10 mg TiO 2 / (Mo 2 C / CdS) powder and the TiO 2 / (Mo 2 C / CdS) films were placed in a mixed solution of lactic acid and deionized water. The volume of the mixed solution was 100 mL, including 90 mL of deionized water solution and 10 mL of lactic acid solution. A 300W xenon lamp with a wavelength of 320 nm to 780 nm was used as a sunlight simulating light source. The irradiation area was 25 cm 2 , working current is 15mA, and illumination time is 1h.

[0087] 3) In this reaction, 10 mg TiO 2 / (Mo 2 C / CdS) powder has a photocatalytic decomposition of water and a hydrogen production rate of 10.7 mmol / h / g under stirring conditions, and a photocatalytic decomposition of water and a hydrogen production rate of 6.1 mmol / h / g under non-stirring conditions. 2 / (Mo 2 The photocatalytic decomposition of water by C / CdS thin films under non-stirring conditions produces hydrogen at rates of 16.0, 16.0 and 15.0 mmol / h / g (corresponding to the hydrogen production rates of films 1, 2 and 3, respectively), all showing more efficient hydrogen production activity than the powder type. Powder-type photocatalysts require continuous stirring during the photocatalytic reaction to achieve uniform light absorption, but this not only increases energy consumption, but also causes solution turbidity, reduced light transmittance, and causes light shielding between particles, thereby affecting the light absorption efficiency. Therefore, powder-type catalysts perform poorly in large-scale hydrogen production and are difficult to separate and process. In contrast, thin-film photocatalysts have higher light absorption efficiency and stability, while avoiding the problem of turbidity in the reaction solution, ensuring that light energy is evenly and directly irradiated to the catalyst surface. In addition, thin-film catalysts are more convenient to recycle, without the need for complex processes such as centrifugation, reflecting their significant advantages in the application of water decomposition to produce hydrogen.

Claims

1. A thin film TiO 2 / (MoP / CdS) composite photocatalyst, Features: The invention comprises a substrate and a TiO2 film attached to the surface of the substrate. 2 / (MoP / CdS) powder photocatalyst, MoP is 1.8%-11.8% (preferably 5%-7%) of the mass of MoP / CdS (Wt%); TiO 2 TiO 2 / (MoP / CdS) mass (Wt%) is 10.0%-50.0% (preferably 25.0%-50.0%).

2. The composite photocatalyst according to claim 1, Features: TiO 2 The MoP / CdS powder photocatalyst is fixed on the surface of the substrate by adhesive to form a layer of TiO 2 / (MoP / CdS) powder photocatalyst thin film layer.

3. The composite photocatalyst according to claim 1 or 2, Features: The substrate is a flat plate of polymethyl methacrylate (PMMA) organic glass, and the adhesive is covered on one side of the organic glass to form an adhesive layer. 2 / (MoP / CdS) powder is evenly spread on the surface of the adhesive layer and fixed to one surface of the organic glass through the adhesive layer.

4. The composite photocatalyst according to claim 1 or 2, Features The adhesive includes one or more of acrylic acid water-based adhesive, acrylate adhesive, or double-sided adhesive; The thickness of the adhesive layer is 100-200μm, 25cm 2 TiO attached to the substrate surface 2 The amount of MoP / CdS powder photocatalyst is 4-14.2 mg (preferably 8-10 mg).

5. A thin film TiO according to any one of claims 1 to 4 2 / (MoP / CdS) composite photocatalyst preparation method, Features: The specific preparation process is as follows: take an area of ​​25cm 2 Clean one side of the surface of the polymethyl methacrylate (PMMA) organic glass, and evenly cover the cleaned side surface with adhesive (with a thickness of 100-200 μm) to form an adhesive layer; Weigh 4-14.2 mg (preferably 8-10 mg) TiO 2 / (MoP / CdS) powder is evenly spread on the surface of the adhesive layer.

6. A TiO 2 / (MoP / CdS) composite photocatalyst preparation method or the thin film TiO 2 / (MoP / CdS) composite photocatalyst preparation method, Features: TiO 2 The TiO / (MoP / CdS) composite photocatalyst was prepared by hydrothermal-calcination method using titanium dioxide, molybdenum phosphide and cadmium nitrate as raw materials. 2 / (MoP / CdS) powder photocatalyst; 1) The specific process of preparing MoP / CdS is as follows: first, according to the mass ratio (Wt%) of MoP to MoP / CdS being 1.8%-11.8% (preferably 5%-7%), weigh the required amount of MoP and CdS, 0.2-0.4g in total, and add them to 20-40mL of absolute ethanol; then, perform ultrasonic treatment for 0.5-2 hours (preferably 0.5-1 hour); stir the above solution, evaporate to dryness, grind, and finally obtain a solid MoP / CdS composite catalyst (particle size range 40-200nm); 2) TiO 2 The specific process of the catalyst is as follows: First, according to the TiO 2 TiO 2 The mass ratio (Wt%) of TiO / (MoP / CdS) is 10.0%-50.0% (preferably 25.0%-50.0%), and the required amount of TiO 2 and MoP / CdS 0.2-0.4g; add the weighed MoP / CdS to 30-60mL ethanol and treat under ultrasonication for 2-3 hours to form suspension A; then, add weighed TiO 2 , and similarly perform ultrasonic treatment for 2-3 hours to form suspension B; add suspension B to suspension A and stir to mix the two evenly; then transfer the mixed solution to a hydrothermal reactor and perform hydrothermal reaction at 110-130°C for 1-4 hours; after the reaction, wash with deionized water and absolute ethanol, and then perform vacuum drying at 60-80°C for 8-24 hours to finally obtain powdered TiO 2 / (MoP / CdS) composite catalyst (particle size range 20-200nm).

7. The preparation method according to claim 6, Features: TiO 2 The specific preparation process is as follows: under magnetic stirring, 2.0-2.5mL (preferably 2.06-2.10mL) of tetrabutyl titanate is added to a solution containing 8-12mL (preferably 10mL) of glycerol and 55-60mL (preferably 58-60mL) of ethanol; after stirring for 20-40 minutes, the mixed solution is transferred to a 100mL Teflon-lined autoclave and subjected to a hydrothermal reaction at 160-200°C (preferably 180-185°C) for 24-25 hours. Then, the obtained white powder is collected, washed with absolute ethanol, and dried at 60-80°C (preferably 60-65°C) for 10-12 hours; The white powder was transferred to an alumina crucible and calcined at 400-500°C (preferably 460-480°C) for 1.0-1.2 hours at a heating rate of 5°C / min. -1 To obtain TiO 2 (particle size range 20-60nm); The specific preparation process of CdS is as follows: First, prepare 0.28 mol / L cadmium nitrate (Cd(NO 3 ) 2 ·4H 2 O) and 0.28 mol / L sodium sulfide (Na 2 S·9H 2 Subsequently, 30 mL of 0.28 mol / L Na 2 S solution was slowly added dropwise to 25 mL, and 0.28 mol / L Cd(NO 3 ) 2 solution; after stirring for 20-40 minutes, the mixed solution is transferred to a 100 mL Teflon-lined autoclave, and a hydrothermal reaction is carried out at 160-200° C. (preferably 180-185° C.) for 24-25 hours; after the reaction is completed, the mixture is centrifuged twice with deionized water and absolute ethanol, and then dried at 60-80° C. (preferably 60-65° C.) for 10-12 hours to obtain CdS (particle size range 40-80 nm); The specific preparation process of MoP is as follows: weigh 199.8-200.6 mg MoO 3 (preferably 199.9-200.1 mg) and 3.9-4.1 g NaH 2 PO 2 -H 2 O (preferably 4.0 g) is mixed evenly and then fully ground. Subsequently, the mixture is transferred to an alumina crucible and calcined at 680-720°C (preferably 700-710°C) for 1-2 hours at a heating rate of 2-5°C / min; after cooling, the obtained black solid is immersed in a 1-2 mol / L HCl solution to remove impurities; finally, it is washed four times with deionized water to achieve neutralization, and then dried at 60-90°C (preferably 75-85°C) for 12-14 hours to obtain MoP (particle size range 50-200 nm).

8. A TiO prepared by the preparation method according to any one of claims 6 to 7 2 / (MoP / CdS) composite photocatalyst.

9. The TiO according to claim 8 2 / (MoP / CdS) composite photocatalyst or any thin film TiO 2 Application of / (MoP / CdS) composite photocatalyst as photocatalyst in photocatalytic water decomposition to produce hydrogen.