Graphite-phase carbon nitride photocatalyst as well as preparation method and application thereof
Modified graphitic carbon nitride photocatalysts were prepared by hydrothermal reaction and high-temperature calcination, which solved the problems of light absorption and carrier recombination in visible light catalytic water splitting to produce hydrogen, and achieved a high-efficiency improvement in photocatalytic performance.
Patent Information
- Application Number
- CN202411518162.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing graphitic carbon nitride photocatalysts suffer from poor light absorption, severe recombination of photogenerated carriers, and small specific surface area in visible light catalytic water splitting for hydrogen production, which limits their photocatalytic performance.
A modified precursor was prepared by hydrothermal reaction using melamine, cyanuric acid and hexamethylenetetramine in a specific ratio as raw materials to form a melamine-cyanuric acid supramolecular structure. Combined with high-temperature calcination, the crystallinity, interlayer spacing and microstructure of graphitic carbon nitride were optimized, thereby enhancing its specific surface area and light absorption capacity.
It significantly improves the specific surface area, light absorption capacity, and photogenerated carrier separation efficiency of graphitic carbon nitride photocatalysts, thereby enhancing the efficiency of visible light photocatalytic hydrogen production, while being low-cost and environmentally friendly.
Smart Images

Figure CN119034789A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photocatalysts, and in particular to a graphite phase carbon nitride photocatalyst and a preparation method and application thereof. Background Art
[0002] At present, the world's energy problems are becoming increasingly severe, and environmental pollution problems need to be solved urgently. It is imperative to use renewable clean energy to replace fossil energy. The field of solar photocatalytic water decomposition to produce hydrogen is booming today, and the development of efficient, stable, environmentally friendly, and low-cost visible light catalysts is the key to promoting the large-scale application of photocatalytic water decomposition to produce hydrogen. Organic semiconductor graphite phase carbon nitride (g-CN) has many advantages such as non-toxicity, pollution-free, and stable chemical and physical properties. It is one of the most promising visible light catalysts. However, its poor visible light absorption, severe photogenerated carrier recombination, and small specific surface area limit its photocatalytic hydrogen production performance. Therefore, it is necessary to improve its visible light catalytic hydrogen production performance by targeted modification of g-CN.
[0003] At present, researchers usually use small molecule doping, element doping, copolymerization, morphology control, crystal structure control and other methods to modify g-CN to improve its photocatalytic activity. Among them, using precursors for small molecule doping and then sintering to prepare graphite phase carbon nitride is an effective strategy, which can change the morphology and component content of g-CN, thereby optimizing the light absorption, carrier transfer and surface reaction ability of g-CN.
[0004] Small molecule doping usually uses hydrothermal and thermal condensation methods to make specific organic matter react with precursors. However, the thermal condensation method is prone to uneven modification and material agglomeration, which is not conducive to improving the performance of photocatalysts. At the same time, it will generate harmful gases such as nitrogen oxides, polluting the environment.
[0005] Finding suitable small molecules for precursor modification is a difficult problem. CN114632535A discloses a graphite-phase carbon nitride photocatalyst for sewage treatment and a preparation method thereof, which specifically discloses the following contents: a new precursor is obtained by hydrothermalizing a mixture of melamine and hexamethylenetetramine in a closed environment, and a modified graphite-phase carbon nitride is obtained after high-temperature calcination; however, the obtained g-CN has a small specific surface area, a poor degree of polymerization, and a low activity improvement relative to that before modification.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The object of the present invention is to provide a method for preparing a graphite phase carbon nitride photocatalyst. The graphite phase carbon nitride photocatalyst prepared by the method has the advantages of low cost, strong light absorption ability, fast photogenerated carrier transfer rate, and high photocatalytic hydrogen production activity. Another object of the present invention is to provide a graphite phase carbon nitride photocatalyst prepared by the above method and its application.
[0008] Specifically, the present invention provides the following technical solutions: The present invention provides a method for preparing a graphite phase carbon nitride photocatalyst, comprising: using melamine, cyanuric acid and hexamethylenetetramine (HMTA) as raw materials, carrying out a hydrothermal reaction, washing, drying, grinding the obtained product, and then calcining at a high temperature; Among them, melamine: cyanuric acid: hexamethylenetetramine = (0.84-4.2) g: (0-4.2) g: (0-1000) mg, and the amounts of cyanuric acid and hexamethylenetetramine are not zero at the same time.
[0009] The present invention finds that a modified precursor can be prepared by hydrothermal reaction of melamine, cyanuric acid and HMTA in a specific ratio, and then the modified precursor is calcined at a high temperature to obtain a graphite phase carbon nitride photocatalyst with excellent effect.
[0010] Specifically, during the hydrothermal reaction, melamine and cyanuric acid self-assemble to form melamine-cyanuric acid supramolecules, which have a huge impact on the crystallinity, interlayer spacing, and crystal orientation of the sintered graphite carbon nitride; at the same time, hexamethylenetetramine changes the microstructure of the precursor with its unique three-dimensional structure, thereby greatly increasing the specific surface area of the sintered graphite carbon nitride; the specific surface area, light absorption capacity, and photogenerated carrier separation efficiency of the finally prepared graphite carbon nitride photocatalyst are significantly enhanced, achieving a further improvement in the efficiency of visible light catalytic hydrogen production.
[0011] Those skilled in the art can set other parameters in the process according to common knowledge, which can all obtain effects equivalent to those described above in the present invention. However, there are also better technical solutions for other process parameters. For this reason, the present invention further explores and obtains the following preferred solutions.
[0012] Preferably, the temperature of the hydrothermal reaction is 100-180°C and the time is 20±5 h; the effect is better when the hydrothermal reaction conditions are controlled within the above range.
[0013] Preferably, the washing is: first washing with deionized water for 3-4 times, and then washing with ethanol for 1-2 times.
[0014] In a specific embodiment, each wash is followed by centrifugation.
[0015] Preferably, the drying is carried out at 60±5° C. and under vacuum conditions for 12±1 h.
[0016] Preferably, the calcination is: heating to 520±10°C at a rate of 5±0.5°C / min and maintaining for 4±0.5 h; the modified precursor is calcined under the above conditions, and the obtained graphite phase carbon nitride photocatalyst has a better effect.
[0017] As a preferred technical solution of the present invention, the preparation method comprises the following steps: (1) Melamine, cyanuric acid and hexamethylenetetramine were added into a hydrothermal reactor containing 30±5 mL of water in sequence, stirred evenly and then subjected to hydrothermal reaction at 100-180°C for 20±5 h. The obtained product was first washed with deionized water for 3-4 times, then washed with ethanol for 1-2 times, and then dried at 60±5°C under vacuum for 12±1 h, and then ground to obtain a precursor; (2) The precursor is heated to 520±10°C at a rate of 5±0.5°C / min, maintained at the temperature for 4±0.5 h, cooled and then ground to obtain the product.
[0018] The present invention modifies a graphite phase carbon nitride precursor based on a co-hydrothermal method. In the hydrothermal reaction, melamine reacts with cyanuric acid to form a melamine-cyanuric acid (MCA) supramolecule, and hexamethylenetetramine is embedded in the supramolecule through hydrogen bonds, thereby jointly realizing the modification of the graphite phase carbon nitride precursor. The modified precursor is sintered to obtain a graphite phase carbon nitride photocatalyst.
[0019] The present invention also provides a graphite phase carbon nitride photocatalyst, which is prepared by the above-mentioned preparation method.
[0020] The present invention also provides the use of the above-mentioned graphite phase carbon nitride photocatalyst in photocatalytic water decomposition to produce hydrogen.
[0021] The present invention also provides a method for producing hydrogen by photocatalytically decomposing water, comprising: dispersing the above-mentioned graphite phase carbon nitride photocatalyst in an aqueous solution of triethanolamine, adding Pt, and carrying out a reaction.
[0022] Preferably, the amount of the graphite-phase carbon nitride photocatalyst is 20±0.5 mg, the amount of the triethanolamine aqueous solution is 40±1 mL, and the volume concentration of the triethanolamine aqueous solution is 10±1%, and the amount of Pt added is 3±0.5% of the graphite-phase carbon nitride photocatalyst.
[0023] Based on the above scheme, the beneficial effects of the present invention are as follows: The photocatalytic hydrogen production test of the graphite phase carbon nitride photocatalyst prepared by the method of the present invention showed that its specific surface area was 264.2 m2 g -1 The maximum hydrogen production activity can reach 1688 μmol h -1 g -1 , which are 46.3 times and 21.6 times of pure g-CN respectively; it can be seen that the graphite phase carbon nitride photocatalyst of the present invention has the advantages of low cost, strong light absorption ability, fast photogenerated carrier transfer speed, and high photocatalytic hydrogen production activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a bar graph of the hydrogen production activity of the photocatalysts in Comparative Example 1 and Examples 1-5.
[0025] Figure 2 It is a bar graph of the hydrogen production activity of the photocatalyst in Comparative Example 1 and Examples 1, 5, 6, and 7.
[0026] Figure 3 It is a bar graph of the hydrogen production activity of the graphite phase carbon nitride photocatalyst in Comparative Example 1 and Examples 1 and 7-12.
[0027] Figure 4 The XRD spectra of the precursors in Comparative Examples 1 and 2 and Examples 1 and 7-12.
[0028] Figure 5 XRD spectra of the photocatalysts in Comparative Example 1 and Examples 1 and 12.
[0029] Figure 6 It is the BET diagram of the photocatalyst in comparative example 1 and embodiments 1 and 12.
[0030] Figure 7 UV-Vis graphs of the photocatalysts in Comparative Example 1 and Examples 1, 8, and 12.
[0031] Figure 8 It is the KM method Tauc plot curve diagram of the photocatalyst in Comparative Example 1 and Examples 1 and 12.
[0032] Fig. 9 Steady-state PL diagrams of the catalysts in Comparative Example 1 and Examples 1 and 12.
[0033] Fig.10 These are the transient PL images of the photocatalysts in Comparative Example 1 and Example 12. DETAILED DESCRIPTION
[0034] The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.
[0035] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.
[0036] Example 1 This embodiment provides a graphite phase carbon nitride photocatalyst, and the preparation method thereof is as follows: Step 1: Weigh 4.2 g of melamine, 0 g of cyanuric acid and 500 mg of hexamethylenetetramine, add them into a 50 mL hydrothermal kettle lining containing 30 mL of water in sequence under stirring, stir for 15 minutes, and preheat the oven to 180°C; Step 2: Place the inner lining of the hydrothermal kettle after stirring in step 1 into a matching stainless steel shell and seal it, then place it in a preheated oven for 20 hours of hydrothermal reaction; Step 3: After the hydrothermal reaction in step 2 is completed, the mixture is naturally cooled to room temperature, and the reaction product is washed with deionized water and centrifuged three times, and washed with ethanol and centrifuged once, and the centrifuge speed is 10000 rpm; Step 4: Place the product obtained by centrifugation in step 3 into an oven and vacuum dry it at 60°C for 12 hours; grind the dried sample into powder and name it M-CA-HT-HMTA-500-180-1; x - T - n middle, x is the mass of HMTA input (mg), T is the treatment temperature (°C), n It is the mass ratio of melamine to the sum of melamine and cyanuric acid in the initial feed (also known as MCA ratio); since the amount of cyanuric acid used is 0, it can also be named M-HT-HMTA-500-180; Step 5: Weigh 2 g of the powder obtained in step 4 and put it into a crucible, put it into a muffle furnace and calcine it in an air atmosphere at a heating rate of 5°C / min, keep it at 520°C for 4 hours and then cool it naturally; the obtained sample is ground into powder and named CN-CA-HT-HMTA-500-180-1; based on CN-CA-HT-HMTA- x - T - n middle, x is the mass of HMTA input in the preparation of the precursor (mg), T is the processing temperature when preparing the precursor (°C), nIt is the mass ratio of melamine to the sum of melamine and cyanuric acid in the initial feed of the precursor (also known as MCA ratio); since the amount of cyanuric acid used is 0, it can also be named CN-HT-HMTA-500-180.
[0037] Example 2 This embodiment provides a graphite-phase carbon nitride photocatalyst, and its preparation method is different from that of Example 1 in that: 3.36 g of melamine, 0.84 g of cyanuric acid, the MCA ratio is 0.8, the precursor is named M-CA-HT-HMTA-500-180-0.8, and the graphite-phase carbon nitride photocatalyst is named CN-CA-HT-HMTA-500-180-0.8.
[0038] Example 3 This embodiment provides a graphite-phase carbon nitride photocatalyst, and its preparation method is different from that of Example 1 in that: 2.52 g of melamine, 1.68 g of cyanuric acid, the MCA ratio is 0.6, the precursor is named M-CA-HT-HMTA-500-180-0.6, and the graphite-phase carbon nitride photocatalyst is named CN-CA-HT-HMTA-500-180-0.6.
[0039] Example 4 This embodiment provides a graphite-phase carbon nitride photocatalyst, and its preparation method is different from that of Example 1 in that: 1.68 g of melamine, 2.52 g of cyanuric acid, the MCA ratio is 0.4, the precursor is named M-CA-HT-HMTA-500-180-0.4, and the graphite-phase carbon nitride photocatalyst is named CN-CA-HT-HMTA-500-180-0.4.
[0040] Example 5 This embodiment provides a graphite-phase carbon nitride photocatalyst, and its preparation method is different from that of Example 1 in that: 0.84 g of melamine, 3.36 g of cyanuric acid, MCA ratio 0.2, the precursor is named M-CA-HT-HMTA-500-180-0.2, and the graphite-phase carbon nitride photocatalyst is named CN-CA-HT-HMTA-500-180-0.2.
[0041] Example 6 This embodiment provides a graphite phase carbon nitride photocatalyst, and the preparation method thereof is as follows: Step 1: Weigh 0.84 g melamine, 3.36 g cyanuric acid and 500 mg hexamethylenetetramine, add them into a 50 mL hydrothermal autoclave lining containing 30 mL water in sequence under stirring, stir for 15 minutes, and preheat the oven to 140°C; Step 2: Place the inner lining of the hydrothermal kettle after stirring in step 1 into a matching stainless steel shell and seal it, then place it in a preheated oven for 20 hours of hydrothermal reaction; Step 3: After the hydrothermal reaction in step 2 is completed, the mixture is naturally cooled to room temperature, and the reaction product is washed with deionized water and centrifuged three times, and washed with ethanol and centrifuged once, and the centrifuge speed is 7000 rpm; Step 4: Place the product obtained by centrifugation in step 3 in an oven and vacuum dry it at 60° C. for 12 hours; grind the dried sample into powder, which is named M-CA-HT-HMTA-500-140-0.2; since the MCA ratio used in the preparation method after this embodiment is 0.2, it can also be named M-CA-HT-HMTA-500-140; Step 5: Weigh 2 g of the powder obtained in step 4 and put it into a crucible, put it into a muffle furnace and calcine it in an air atmosphere at a heating rate of 5°C / min, keep it at 520°C for 4 hours and then cool it naturally; the obtained sample is ground into powder and named CN-CA-HT-HMTA-500-140-0.2; since the MCA ratio used in the preparation method after this embodiment is 0.2, it can also be named CN-CA-HT-HMTA-500-140.
[0042] Example 7 This embodiment provides a graphite-phase carbon nitride photocatalyst, and its preparation method is different from that of Example 6 in that the hydrothermal temperature is 100°C, the precursor is named M-CA-HT-HMTA-500-100, and the graphite-phase carbon nitride photocatalyst is named CN-CA-HT-HMTA-500-100.
[0043] Example 8 This embodiment provides a graphite phase carbon nitride photocatalyst, and the preparation method thereof is as follows: Step 1: Weigh 0.84 g melamine, 3.36 g cyanuric acid and 0 mg hexamethylenetetramine, add them into a 50 mL hydrothermal autoclave lining containing 30 mL water in sequence under stirring, stir for 15 minutes, and preheat the oven to 100 °C; Step 2: Place the inner lining of the hydrothermal kettle after stirring in step 1 into a matching stainless steel shell and seal it, then place it in a preheated oven for 20 hours of hydrothermal reaction; Step 3: After the hydrothermal reaction in step 2 is completed, the mixture is naturally cooled to room temperature, and the reaction product is washed with deionized water and centrifuged three times, and washed with ethanol and centrifuged once, and the centrifuge speed is 7000 rpm; Step 4: Place the product obtained by centrifugation in step 3 into an oven and vacuum dry it at 60°C for 12 hours; grind the dried sample into powder, named M-CA-HT-HMTA-0-100; Step 5: Weigh 2 g of the powder obtained in step 4 and put it into a crucible, which is then placed in a muffle furnace and calcined in an air atmosphere at a heating rate of 5°C / min. Keep the mixture at 520°C for 4 hours and then cool it naturally. Grind the obtained sample into powder and name it CN-CA-HT-HMTA-0-100.
[0044] Example 9 This embodiment provides a graphite-phase carbon nitride photocatalyst, and its preparation method is different from that of Example 8 in that: the amount of hexamethylenetetramine used is 10 mg, the precursor is named M-CA-HT-HMTA-10-100, and the graphite-phase carbon nitride photocatalyst is named CN-CA-HT-HMTA-10-100.
[0045] Example 10 This embodiment provides a graphite-phase carbon nitride photocatalyst, and its preparation method is different from that of Example 8 in that: the amount of hexamethylenetetramine used is 50 mg, the precursor is named M-CA-HT-HMTA-50-100, and the graphite-phase carbon nitride photocatalyst is named CN-CA-HT-HMTA-50-100.
[0046] Embodiment 11 This embodiment provides a graphite-phase carbon nitride photocatalyst, and its preparation method is different from that of Example 8 in that: the amount of hexamethylenetetramine used is 100 mg, the precursor is named M-CA-HT-HMTA-100-100, and the graphite-phase carbon nitride photocatalyst is named CN-CA-HT-HMTA-100-100.
[0047] Example 12 This embodiment provides a graphite-phase carbon nitride photocatalyst, and its preparation method is different from that of Example 8 in that: the amount of hexamethylenetetramine used is 200 mg, the precursor is named M-CA-HT-HMTA-200-100, and the graphite-phase carbon nitride photocatalyst is named CN-CA-HT-HMTA-200-100.
[0048] Comparative Example 1 This comparative example provides a photocatalyst, and its preparation method is as follows: Step 1: Place commercially available melamine in an oven and vacuum dry it at 60°C for 12 hours. Grind the dried sample into powder, named M. Step 2: Weigh 2 g of the powder obtained in step 1 and put it into a crucible, which is then placed in a muffle furnace for calcination at a heating rate of 5°C / min. Keep the mixture at 520°C for 4 hours and then cool it naturally. Grind the obtained sample into powder and name it CN.
[0049] Comparative Example 2 This comparative example provides a graphite phase carbon nitride photocatalyst, and its preparation method is as follows: Step 1: Weigh 4.2 g of melamine and 500 mg of hexamethylenetetramine, add them into a 50 mL hydrothermal autoclave lining containing 30 mL of water in sequence while stirring, stir for 15 minutes, and preheat the oven to 100 °C; Step 2: Place the inner lining of the hydrothermal kettle after stirring in step 1 into a matching stainless steel shell and seal it, then place it in a preheated oven for 20 hours of hydrothermal reaction; Step 3: After the hydrothermal reaction in step 2 is completed, the mixture is naturally cooled to room temperature, and the reaction product is washed with deionized water and centrifuged three times, and washed with ethanol and centrifuged once, and the centrifuge speed is 7000 rpm; Step 4: Place the product obtained by centrifugation in step 3 into an oven and vacuum dry it at 60°C for 12 hours; grind the dried sample into powder, named M-HT-HMTA-500-100; Step 5: Weigh 2 g of the powder obtained in step 4 and put it into a crucible, which is then placed in a muffle furnace for calcination at a heating rate of 5°C / min. Keep the mixture at 520°C for 4 hours and then cool it naturally. Grind the obtained sample into powder and name it CN-HT-HMTA-500-100.
[0050] Performance Evaluation Figure 1 The graph is a bar graph of the hydrogen production activity of the photocatalysts in Comparative Example 1 and Examples 1-5, wherein the test method for photocatalytic water decomposition to produce hydrogen includes: taking 20 mg of the photocatalyst and dispersing it in 40 mL of a 10 vol% triethanolamine solution, adding Pt (3 wt% of the photocatalyst) as a co-catalyst, and detecting the amount of hydrogen produced in the photocatalytic system. Figure 1 It can be seen that with the increase of the proportion of cyanuric acid in the precursor hydrothermal, the hydrogen production activity of sintered g-CN gradually increased, and the highest activity was reached when the MCA ratio was 0.2, reaching 802 μmol h -1 g -1 .
[0051] Figure 2 The bar graph of the hydrogen production activity of the photocatalyst in Comparative Example 1 and Examples 1, 5, 6, and 7 shows that the hydrothermal temperature of the precursor was adjusted based on the optimal MCA ratio of 0.2. Figure 2It can be seen that the hydrogen production activity increases with the decrease of hydrothermal temperature. When the hydrothermal temperature is 100 °C, the hydrogen production activity is the highest, reaching 1110 μmol h -1 g -1 .
[0052] Figure 3 The bar graph of the hydrogen production activity of the photocatalysts in Comparative Example 1 and Examples 1 and 7-12 shows that the content of HMTA doped in the precursor was adjusted based on the optimal MCA ratio of 0.2 and the optimal hydrothermal temperature of 100°C. Figure 3 It can be seen that with the increase of HMTA doping amount, the photocatalytic hydrogen production activity of the sintered g-CN first increased and then decreased, indicating that after the introduction of cyanuric acid in the precursor, HMTA can still effectively improve the performance of the sintered g-CN. The highest activity is 1688 μmol h-1 at a doping amount of 200 mg. -1 g -1 .
[0053] Figure 4 The XRD spectra of the precursors in Comparative Examples 1 and 2 and Examples 1 and 7-12 are shown in Table 1. Figure 4 It can be seen that no matter how much HMTA is added, the characteristic peaks of MCA supramolecules, melamine and cyanuric acid (CA) are present at the same time, indicating that MCA supramolecules are generated during the reaction, and both melamine and cyanuric acid remain after the reaction. At the same time, the conversion of melamine and cyanuric acid cannot occur under 100℃ hydrothermal conditions, but melamine and cyanuric acid can self-assemble to form MCA supramolecules under 100℃ hydrothermal conditions.
[0054] Figure 5 The XRD spectra of the photocatalysts in Comparative Example 1 and Examples 1 and 12 are shown in Table 1. Figure 5 It can be seen that the intensity of the peak at 12.9° of CN-CA-HT-HMTA-200-100 is significantly reduced relative to that at 27.8°, indicating that the introduction of cyanuric acid in the precursor has a great influence on the crystallinity, interlayer spacing, and crystal orientation of g-CN.
[0055] Figure 6 The BET diagrams of the photocatalysts of Comparative Example 1 and Examples 1 and 12 are shown in Table 1. Figure 6 It can be seen that the specific surface area of the CN-CA-HT-HMTA-200-100 sample (264.2 m 2 g -1 ) is greatly improved, which is CN (5.7 m 2 g -1 ) is 46.3 times that of CN-HT-HMTA-500-180 (29.4m 2 g -1) is 9.0 times that of the sintered g-CN, indicating that the introduction of CA in the precursor can change the specific surface area of the sintered g-CN.
[0056] Figure 7 The UV-Vis graphs of the photocatalysts in Comparative Example 1 and Examples 1 and 12 are shown in Table 1. Figure 7 It can be seen that the visible light absorption performance of the sample doped with HMTA in the precursor is significantly enhanced, indicating that the introduction of HMTA increases the defects of the sintered g-CN.
[0057] Figure 8 The KM method Tauc plot curves of the photocatalysts of Comparative Example 1 and Examples 1 and 12 are shown in Table 1. Figure 8 It can be seen that after adding CA, the absorption edge of the precursor sintering blue-shifts and the band gap becomes wider. The band gap of CN-CA-HT-HMTA-200-180 is 2.52 eV, indicating that the introduction of CA and HMTA in the precursor changes the band structure of g-CN.
[0058] Fig. 9 The steady-state PL diagrams of the photocatalysts of Comparative Example 1 and Examples 1 and 12 are shown in Table 1. Fig. 9 It can be seen that the recombination peak of CN-CA-HT-HMTA-200-100 is lower than that of CN-HT-HMTA-500-180, indicating that the introduction of cyanuric acid into the precursor is beneficial to inhibiting the recombination of the sintered g-CN carriers.
[0059] Fig.10 The transient PL graphs of the photocatalysts of Comparative Example 1 and Example 12 are shown in Table 1. Fig.10 It can be seen that the average carrier lifetime of the CN-CA-HT-HMTA-200-100 sample is lower than that of the CN sample. Fig. 9 The recombination peak of the CN-CA-HT-HMTA-200-100 sample is lower than that of CN, which can be inferred that the reduction in the average carrier lifetime is caused by the enhanced non-radiative recombination of photogenerated carriers. This shows that after the introduction of HMTA and CA into the precursor, the transfer speed of photogenerated carriers in the sintered g-CN is faster, which is conducive to the occurrence of photocatalytic reactions.
[0060] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A method for preparing a graphite phase carbon nitride photocatalyst, characterized in that: include: Using melamine, cyanuric acid and hexamethylenetetramine as raw materials, a hydrothermal reaction is carried out, and the obtained product is washed, dried, ground, and then calcined at high temperature; Among them, melamine: cyanuric acid: hexamethylenetetramine = (0.84-4.2) g: (0-4.2) g: (0-1000) mg, and the amounts of cyanuric acid and hexamethylenetetramine are not zero at the same time.
2. The preparation method according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 100-180°C and the time is 20±5 h.
3. The preparation method according to claim 1, characterized in that: The washing step is: first washing with deionized water for 3-4 times, and then washing with ethanol for 1-2 times.
4. The preparation method according to claim 1, characterized in that: The drying is performed at 60±5° C. and vacuum conditions for 12±1 h.
5. The preparation method according to claim 1, characterized in that: The calcination is as follows: heating to 520±10°C at a rate of 5±0.5°C / min and maintaining for 4±0.5 h.
6. The preparation method according to claim 1, characterized in that: The steps include: (1) Melamine, cyanuric acid and hexamethylenetetramine were added into a hydrothermal reactor containing 30±5 mL of water in sequence, stirred evenly and then subjected to hydrothermal reaction at 100-180°C for 20±5 h. The obtained product was first washed with deionized water for 3-4 times, then washed with ethanol for 1-2 times, and then dried at 60±5°C under vacuum for 12±1 h, and then ground to obtain a precursor; (2) The precursor is heated to 520±10°C at a rate of 5±0.5°C / min, maintained at the temperature for 4±0.5 h, cooled, and then ground to obtain the product.
7. A graphite phase carbon nitride photocatalyst, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the graphite phase carbon nitride photocatalyst according to claim 7 in photocatalytic water decomposition to produce hydrogen.
9. A method for producing hydrogen by photocatalytic decomposition of water, characterized in that: include: The graphite-phase carbon nitride photocatalyst according to claim 7 is dispersed in an aqueous solution of triethanolamine, and Pt is added to carry out a reaction.
10. The method according to claim 9, characterized in that The amount of the graphite phase carbon nitride photocatalyst is 20±0.5 mg, the amount of the triethanolamine aqueous solution is 40±1 mL, and the volume concentration of the triethanolamine aqueous solution is 10±1%, and the added amount of Pt is 3±0.5% of the graphite phase carbon nitride photocatalyst.
Citation Information
Patent Citations
Preparation method for multi-hole carbon nitride photocatalytic material doped with sulphur
CN103861632A
Hollow tubular g-C3N4 photocatalyst and preparation method and application thereof
CN109806901A
Preparation method of filamentous carbon nitride and product and application thereof
CN110170330A
Double-vacancy graphite phase carbon nitride photocatalyst and preparation method thereof
CN113908872A
Graphite-phase carbon nitride photocatalyst for photocatalytic hydrogen production and preparation method thereof
CN114367299A
Cited By
Porous tubular graphite phase carbon nitride, photocatalyst and preparation method and application of porous tubular graphite phase carbon nitride
CN120423502A