Casting technology of diversified control performance valve casting capable of preventing core breakage
The problem of core fracture was solved by using hollow steel pipes filled with coated sand in the second core of the control performance valve casting, which enhanced the overall strength and quality of the casting and is suitable for casting high-end hydraulic valve bodies.
Patent Information
- Application Number
- CN202411216309.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-29
AI Technical Summary
The core in the casting of the control performance valve is prone to breakage during use, and existing technologies cannot effectively solve this problem, resulting in the persistent issue of core breakage.
Hollow steel pipes were used to replace the second core, and coated sand was filled inside to form an internal filling layer, which enhanced the support strength and prevented breakage.
It effectively enhances the overall strength of the casting, prevents core breakage, improves the quality and reliability of the casting, and meets the technical requirements of high-end hydraulic valve bodies.
Smart Images

Figure CN119035458A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of casting of diversified control performance valve castings, and in particular to diversified control performance valve castings and a casting process. Background Art
[0002] As a key component in the hydraulic pumping system of an excavator, the diversified control performance valve casting has the advantages of high integration, strong reliability, and long life. Based on the fact that multiple flow channels are set in the control performance valve casting, it is necessary to set multiple mud cores in the casting mold to realize the shape of the flow channels.
[0003] Due to the small inner diameter of the flow channel, the inner diameter of the mud core in the direct casting mold is small, which will directly lead to the problem of mold core breakage after long-term use. However, since it is generally impossible to place core bones in mud cores with small diameters, and conventional core supports cannot be used, simply increasing the strength of the coated sand can no longer solve the core breakage problem, which leads to the continued existence of the core breakage problem in the control performance valve casting mold. Summary of the invention
[0004] The invention discloses a casting process for a diversified control performance valve casting capable of preventing core breakage, aiming to solve the technical problem of the persistent problem of core breakage in a control performance valve casting mold.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A casting process for a valve casting with diversified control performance and capable of preventing core breakage, comprising the following specific steps:
[0007] S1: Product simulation: Determine the mold making process by simulating the casting;
[0008] S2: Product trial production: Make a casting mold based on the manufacturing process of the casting mold body;
[0009] S3: Casting: pouring liquid metal into the mold and taking it out after cooling and forming;
[0010] S4: Subsequent processing: polish the surface of the removed casting and inspect its size and surface quality;
[0011] The casting mold in S1 includes a casting mold body, the casting mold body includes a first mud core and a second mud core, and the second mud core is made of a hollow steel pipe. The casting in S3 includes a casting body, a plurality of flow channels are arranged in the casting body, and flow channel openings are respectively arranged at both ends of each flow channel, and the plurality of flow channel openings correspond to the positions of the plurality of first mud cores and the second mud cores.
[0012] Due to the small inner diameter of the mud core in the mold, it is generally impossible to place core bones in the first mud core and the second mud core, and conventional core supports cannot be used. Simply increasing the strength of the coated sand can no longer solve the core breakage problem. Therefore, by replacing the second mud core with a hollow steel pipe material, the supporting strength of the second mud core is greatly enhanced. The strengthened second mud core can provide sufficient support to avoid fracture, thereby effectively enhancing the overall strength of the casting and perfectly solving the defect of core breakage.
[0013] In a preferred solution, the second mud core is filled with an internal filling layer, and the internal filling layer is composed of coated sand.
[0014] By filling the second mud core with an internal filling layer, if the length of the second mud core is long, the mud core made of the steel pipe may be deformed after long-term use. Therefore, by filling the second mud core with an internal filling layer and filling the second mud core with coated sand, the supporting strength of the hollow steel pipe can be optimized, and at the same time, it can also effectively prevent the steel pipe from dissolving and causing water penetration.
[0015] In a preferred embodiment, S1 comprises the following specific steps:
[0016] S11: Determine the basic process before product mold opening;
[0017] S12: simulate the solidification process of molten iron in the process;
[0018] S13: Prediction of shrinkage cavity position in castings;
[0019] S14: Determine the basic process: According to the simulation results, the molding process adopts the automatic molding line core dropping, and the mud core is formed by hot core box coated sand without shell;
[0020] The S2 comprises the following specific steps:
[0021] S21: first sample;
[0022] S22: second sample;
[0023] S23: the third sample;
[0024] S24: Determine the casting process;
[0025] The S21 includes the following specific steps:
[0026] S211: Core making: Since the product flow channel is small and the core bone cannot be placed, the mud core uses CER50 coated sand and the coating uses 413 coating;
[0027] S212: Modeling;
[0028] S213: First inspection: The first sample is placed on the clamping platform. Through the inspection of the first sample, it is found that the flow channel of the casting is broken;
[0029] The S22 comprises the following specific steps:
[0030] S221: Replace the mud core and repeat the sample: Repeat S211 to S212, and change the mud core from CER50 coated sand to 290 ultra-high strength sand;
[0031] S222: Second inspection: The second sample is placed on the clamping platform. Through the inspection of the second sample, it is found that the casting flow channel still has fractures, and the fracture position is the same as that of the first sample;
[0032] The S23 comprises the following specific steps:
[0033] S231: Modify the mud core molding method and repeat the test: In the second test, it was analyzed that the mud core flow channel was broken. This was because the size of the broken flow channel of the casting was small, with a hole diameter of only 4mm. The strength of the coated sand was not enough to place the core bone. Therefore, the mud core was changed to hollow steel pipe molding;
[0034] S232: The third test: The third sample is placed on the clamping platform. Through the inspection of the third sample, it is found that the appearance of the casting meets the technical requirements, and the flow channel has no sand adhesion, deformation or fracture defects.
[0035] After determining the basic process of castings through product simulation and trial production, the samples are made multiple times and tested one by one to analyze them one by one. The mud core and coating materials are replaced through the second and third samples. The casting process of the casting is determined through repeated tests. Under this process, defects can be more easily controlled and resolved to better obtain a higher-quality casting process. The development of this casting process has laid a good foundation for improving the technical level of its own high-end hydraulic valve body castings, meeting the needs of domestic high-end hydraulic valve users, and replacing imported valves. It has great practical significance for changing the situation of poor precision and low technical content of similar domestic castings, as well as for expanding domestic and foreign market shares in the future.
[0036] In a preferred embodiment, the clamping platform includes a base, and the top of the base is simultaneously connected to two groups of base frames, one group of base frames is fixedly connected to the base, and the other group of base frames is movably connected to the base, the inner wall of each group of the base frames is fixedly connected to a hydraulic rod through a support frame, and the output end of the hydraulic rod is fixedly connected to a second support plate, the top of the second support plate is connected to the first support plate through a spring, the bottom end of the first support plate is fixedly connected to a plurality of limit rods, and the plurality of limit rods are movably inserted in the second support plate, the top of the first support plate is hinged to two connecting rods, the same end of each of the connecting rods is hinged to a slider, and the top of the slider is fixedly connected to a clamping block, the top of each group of the base frames is fixedly connected to a placing table, and a slide groove is provided on the placing table, and the slide block is movably connected in the slide groove.
[0037] By providing a clamping platform, when performing strength testing on castings, the valve body casting to be tested can be first placed on the clamping platform, and the two ends of the casting can be placed on different placement platforms respectively. When the hydraulic rod retracts, a stable clamping force is provided to the clamping block, so that it can stably clamp the two ends of the casting, and the middle section of the casting is suspended in the air. In this way, the testing process can be accelerated and the time required for testing can be saved during the strength testing process. Based on the setting of the slide rail, the distance between the two base frames can be changed to adapt to the use of castings of different lengths.
[0038] As can be seen from the above, a casting process for a valve casting with diversified control performance that can prevent core breakage includes the following specific steps: S1: product simulation: determine the manufacturing process of the casting mold by simulating the casting; S2: product trial production: make a casting mold based on the manufacturing process of the casting mold body; S3: casting molding: pour liquid metal into the casting mold, and take it out after cooling and molding; S4: subsequent processing: polish the surface of the taken out casting, and inspect its size and surface quality, the casting mold in S1 includes a casting mold body, the casting mold body includes a first mud core and a second mud core, and the second mud core is made of a hollow steel pipe, the casting in S3 includes a casting body, a plurality of flow channels are arranged in the casting body, and flow channel openings are respectively arranged at both ends of each flow channel, and the plurality of flow channel openings correspond to the positions of the plurality of first mud cores and second mud cores. The casting process for a valve casting with diversified control performance that can prevent core breakage provided by the present invention has the technical effect of effectively enhancing the overall strength of the casting and perfectly solving the defect of core breakage. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 A schematic diagram of the internal structure of a casting mold for a casting process of a valve casting with diversified control performance that can prevent core breakage proposed by the present invention.
[0040] Figure 2 This is a schematic diagram of the internal structure of the second mud core in a casting mold of a casting process for a valve casting with diversified control performance that can prevent core breakage proposed by the present invention.
[0041] Figure 3 This is a cross-sectional view of a casting body of a casting process for a valve casting with diversified control performance that can prevent core breakage, as proposed by the present invention, and position A is the fracture position.
[0042] Figure 4 This is a schematic diagram of the clamping platform structure of a casting process for a valve casting with diversified control performance that can prevent core breakage, as proposed by the present invention.
[0043] Figure 5 This is a schematic diagram of the structure of the clamping platform portion of a casting process for a valve casting with diversified control performance that can prevent core breakage, as proposed by the present invention.
[0044] Figure 6 The present invention provides a flow chart of a casting process for a valve casting with diversified control performances capable of preventing core breakage.
[0045] In the figure: 1, mold body; 2, first mud core; 3, second mud core; 4, internal filling layer; 5, casting body; 6, flow channel opening; 7, flow channel;
[0046] 8. Base; 9. Slide rail; 10. Slide seat; 11. Base frame; 12. Support frame; 13. Hydraulic rod; 14. Placement table; 15. Clamping block; 16. Slide groove; 17. Sliding block; 18. Connecting rod; 19. First support plate; 20. Spring; 21. Second support plate; 22. Limiting rod. DETAILED DESCRIPTION
[0047] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0048] The present invention discloses a casting process for a diversified control performance valve casting capable of preventing core breakage, which is mainly used in the casting scenario of performance valve castings.
[0049] Reference Figure 1-Figure 6 A casting process for a valve casting with diversified control performance and capable of preventing core breakage comprises the following specific steps:
[0050] S1: Product simulation: Determine the mold making process by simulating the casting;
[0051] S2: Product trial production: Make a casting mold based on the manufacturing process of the casting mold body;
[0052] S3: Casting: pouring liquid metal into the mold and taking it out after cooling and forming;
[0053] S4: Subsequent processing: polish the surface of the removed casting and inspect its size and surface quality;
[0054] The mold in S1 includes a mold body 1, which includes a first mud core 2 and a second mud core 3, and the second mud core 3 is made of a hollow steel tube. The casting in S3 includes a casting body 5, and a plurality of flow channels 7 are arranged in the casting body 5, and flow channel openings 6 are respectively arranged at both ends of each flow channel 7, and the plurality of flow channel openings 6 correspond to the positions of the plurality of first mud cores 2 and second mud cores 3. Since the inner diameter of the mud core in the mold body 1 is small, it is generally impossible to place core bones in the first mud core 2 and the second mud core 3, and conventional core supports cannot be used. Simply increasing the strength of the coated sand cannot solve the core breakage problem. Therefore, by replacing the second mud core 3 with a hollow steel tube material, the support strength of the second mud core 3 is greatly enhanced, such as Figure 3 As shown, the reinforced second clay core 3 can provide sufficient support to avoid fracture at position A, thereby effectively enhancing the overall strength of the casting and effectively solving the defect of core breakage.
[0055] Reference Figure 2 In a preferred embodiment, the second mud core 3 is filled with an internal filling layer 4, and the internal filling layer 4 is made of coated sand. If the second mud core 3 is long, the mud core made of steel pipe may be deformed after long-term use. Therefore, the internal filling layer 4 is filled in the second mud core 3. By filling the coated sand in the second mud core 3, the supporting strength of the hollow steel pipe can be optimized, and the dissolution of the steel pipe and water penetration can be effectively prevented.
[0056] Reference Figure 6 In a preferred embodiment, S1 includes the following specific steps:
[0057] S11: Determine the basic process before product mold opening;
[0058] S12: simulate the solidification process of molten iron in the process;
[0059] S13: Prediction of shrinkage cavity position in castings;
[0060] S14: Determine the basic process: According to the simulation results, the molding process adopts the automatic molding line core dropping, and the mud core is formed by hot core box coated sand without shell.
[0061] Reference Figure 6 In a preferred embodiment, S2 includes the following specific steps:
[0062] S21: first sample;
[0063] S22: second sample;
[0064] S23: the third sample;
[0065] S24: Determine the casting process;
[0066] S21 includes the following specific steps:
[0067] S211: Core making: Since the product flow channel is small and the core bone cannot be placed, the mud core uses CER50 coated sand and the coating uses 413 coating;
[0068] S212: Modeling;
[0069] S213: First inspection: The first sample is placed on the clamping platform. By inspecting the first sample, it is found that the casting flow channel is broken.
[0070] Reference Figure 6 In a preferred embodiment, S22 includes the following specific steps:
[0071] S221: Replace the mud core and repeat the sample: Repeat S211 to S212, and change the mud core from CER50 coated sand to 290 ultra-high strength sand;
[0072] S222: Second inspection: The second sample is placed on the clamping platform. Through the inspection of the second sample, it is found that the casting flow channel still has fractures, and the fracture position is the same as that of the first sample;
[0073] S23 includes the following specific steps:
[0074] S231: Modify the mud core molding method and repeat the test: In the second test, it was analyzed that the mud core flow channel was broken. This was because the size of the broken flow channel of the casting was small, with a hole diameter of only 4mm. The strength of the coated sand was not enough to place the core bone. Therefore, the mud core was changed to hollow steel pipe molding;
[0075] S232: The third test: The third sample is placed on the clamping platform. Through the inspection of the third sample, it is found that the appearance of the casting meets the technical requirements, and there is no sand sticking, deformation or fracture defects in the flow channel. After the basic process of the casting is determined through product simulation and trial production, the samples are made many times and tested one by one to analyze the samples one by one. The mud core and coating materials are replaced by the second and third samples. The casting process of the casting is determined after repeated tests. Under this process, it is easier to control and solve defects, so as to better obtain a better casting process. The development of this casting process has laid a good foundation for improving the technical level of its own high-end hydraulic valve body castings and meeting the needs of domestic high-end hydraulic valve users, replacing imported valves. It has great practical significance for changing the situation of poor precision and low technical content of similar domestic castings, as well as for expanding domestic and foreign market shares in the future.
[0076] Reference Figure 4 and Figure 5 In a preferred embodiment, the clamping platform includes a base 8, and the top of the base 8 is simultaneously connected to two groups of base frames 11, one group of base frames 11 is fixedly connected to the base 8, and the other group of base frames 11 is movably connected to the base 8, and the inner wall of each group of base frames 11 is fixedly connected to a hydraulic rod 13 through a support frame 12, and the output end of the hydraulic rod 13 is fixedly connected to a second support plate 21.
[0077] Reference Figure 4 and Figure 5 In a preferred embodiment, the top end of the second support plate 21 is connected to the first support plate 19 through a spring 20, and the bottom end of the first support plate 19 is fixedly connected to a plurality of limit rods 22, and the plurality of limit rods 22 are movably inserted into the second support plate 21, and the top end of the first support plate 19 is hinged with two connecting rods 18.
[0078] Reference Figure 4 and Figure 5 In a preferred embodiment, a slider 17 is hinged to the same end of each connecting rod 18, and a clamping block 15 is fixedly connected to the top of the slider 17. A placement table 14 is fixedly connected to the top of each group of base frames 11, and a slide groove 16 is provided on the placement table 14. The slider 17 is movably connected to the slide groove 16. When the strength test of the casting is performed, the valve body casting to be tested can be placed on the clamping platform first, and the two ends of the casting are placed on different placement tables 14 respectively. When the hydraulic rod 13 is retracted, the valve body casting can be placed on the clamping platform first, and the two ends of the casting can be ... The first support plate 19 is driven downward by the second support plate 21. When the clamping block 15 is clamped on both sides of the casting along the slide groove 16, the continuous retraction of the hydraulic rod 13 and the pulling force of the spring 20 provide a stable clamping force for the clamping block 15, so that it can stably clamp the two ends of the casting, and the middle section of the casting is suspended in the air. Therefore, during the strength test, the test process can be accelerated and the time required for the test can be saved. Based on the setting of the slide rail 9, the distance between the two base frames 11 can be changed to adapt to the use of castings of different lengths.
[0079] Working principle: Due to the small inner diameter of the mud core in the mold body 1, it is generally impossible to place core bones in the first mud core 2 and the second mud core 3, and conventional core supports cannot be used. Simply increasing the strength of the coated sand cannot solve the core breakage problem. Therefore, by replacing the second mud core 3 with a hollow steel pipe material, the support strength of the second mud core 3 is greatly enhanced. Figure 3 As shown, the reinforced second mud core 3 can provide sufficient support to avoid fracture at position A, thereby effectively enhancing the overall strength of the casting and effectively solving the defect of core breakage. If the second mud core 3 is longer, the mud core made of steel pipe may be deformed after long-term use. Therefore, an internal filling layer 4 is filled in the second mud core 3. By filling the second mud core 3 with coated sand, the support strength of the hollow steel pipe can be optimized, and water penetration caused by the dissolution of the steel pipe can be effectively prevented.
[0080] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A casting process for a valve casting with diversified control performance that can prevent core breakage, characterized in that: The specific steps include: S1: Product simulation: Determine the mold making process by simulating the casting; S2: Product trial production: Make a casting mold based on the manufacturing process of the casting mold body; S3: Casting: pouring liquid metal into the mold and taking it out after cooling and forming; S4: Subsequent processing: polish the surface of the removed casting and inspect its size and surface quality; The casting mold in S1 comprises a casting mold body (1), wherein the casting mold body (1) comprises a first mud core (2) and a second mud core (3), and the second mud core (3) is made of a hollow steel pipe. The casting in S3 comprises a casting body (5), wherein a plurality of flow channels (7) are arranged in the casting body (5), and each flow channel (7) is respectively provided with flow channel openings (6) at both ends, and the plurality of flow channel openings (6) correspond to the positions of the plurality of first mud cores (2) and the second mud cores (3).
2. The casting process of a valve casting with diversified control performance capable of preventing core breakage according to claim 1, characterized in that: The second mud core (3) is filled with an internal filling layer (4), and the internal filling layer (4) is formed by coated sand.
3. The casting process of a valve casting with diversified control performance capable of preventing core breakage according to claim 1, characterized in that: The S1 comprises the following specific steps: S11: Determine the basic process before product mold opening; S12: simulate the solidification process of molten iron in the process; S13: Prediction of shrinkage cavity position in castings; S14: Determine the basic process: According to the simulation results, the molding process adopts the automatic molding line core dropping, and the mud core is formed by hot core box coated sand without shell.
4. The casting process of a valve casting with diversified control performance capable of preventing core breakage according to claim 1, characterized in that: The S2 comprises the following specific steps: S21: first sample; S22: second sample; S23: the third sample; S24: Determine the casting process; The S21 includes the following specific steps: S211: Core making: Since the product flow channel size is small and the core bone cannot be placed, the mud core uses CER50 coated sand and the coating uses 413 coating; S212: Modeling; S213: First inspection: The first sample is placed on the clamping platform. By inspecting the first sample, it is found that the casting flow channel is broken.
5. The casting process of a valve casting with diversified control performance capable of preventing core breakage according to claim 4, characterized in that: The S22 comprises the following specific steps: S221: Replace the mud core and repeat the sample: Repeat S211 to S212, and change the mud core from CER50 coated sand to 290 ultra-high strength sand; S222: Second inspection: The second sample is placed on the clamping platform. Through the inspection of the second sample, it is found that the casting flow channel is still broken, and the fracture position is the same as that of the first sample.
6. The casting process of a valve casting with diversified control performance capable of preventing core breakage according to claim 5, characterized in that: The S23 comprises the following specific steps: S231: Modify the mud core molding method and repeat the test: In the second test, it was analyzed that the mud core flow channel was broken. This was because the size of the broken flow channel of the casting was small, and the strength of the coated sand was not enough to place the core bone. Therefore, the mud core was changed to hollow steel pipe molding; S232: The third test: The third sample is placed on the clamping platform. Through the inspection of the third sample, it is found that the appearance of the casting meets the technical requirements, and the flow channel has no sand adhesion, deformation or fracture defects.
7. The casting process of a valve casting with diversified control performance capable of preventing core breakage according to claim 6, characterized in that: The clamping platform comprises a base (8), and the top of the base (8) is simultaneously connected to two groups of base frames (11), one group of base frames (11) is fixedly connected to the base (8), and the other group of base frames (11) is movably connected to the base (8), the inner wall of each group of base frames (11) is fixedly connected to a hydraulic rod (13) via a support frame (12), and the output end of the hydraulic rod (13) is fixedly connected to a second support plate (21).
8. The casting process of a valve casting with diversified control performance capable of preventing core breakage according to claim 7, characterized in that: The top end of the second support plate (21) is connected to the first support plate (19) via a spring (20); the bottom end of the first support plate (19) is fixedly connected to a plurality of limit rods (22), and the plurality of limit rods (22) are movably inserted into the second support plate (21); the top end of the first support plate (19) is hinged to two connecting rods (18).
9. The casting process of a valve casting with diversified control performance capable of preventing core breakage according to claim 8, characterized in that: A slider (17) is hingedly connected to the same end of each connecting rod (18), and the top of the slider (17) is fixedly connected to a clamping block (15). The top of each group of the base frames (11) is fixedly connected to a placement table (14), and a slide groove (16) is provided on the placement table (14), and the slider (17) is movably connected in the slide groove (16).