Online monitoring and closing method and system for melt additive manufacturing pores of laser powder bed
Through the electromagnetic eddy current monitoring and attention mechanism, the Unet++ network combined with in-situ laser impact means, the online monitoring and elimination of pores during the melt additive manufacturing process of laser powder bed is achieved, and the problem of difficulty in effectively removing internal pore defects in the prior art is solved. , improves manufacturing quality and accuracy.
Patent Information
- Application Number
- CN202411211431.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-29
AI Technical Summary
It is difficult to effectively monitor and eliminate internal pore defects in the laser powder bed melt additive manufacturing process. The existing technology mainly relies on offline detection and process parameter optimization, and cannot guarantee the quality of each part.
The electromagnetic eddy current monitoring probe is used to collect eddy current images in real time, extract the stomatal defect characteristics through the Unet++ network integrated with the attention mechanism, and close the stomatal using in-situ laser impact means, and adjust the laser power, spot diameter, pulse width and scanning tracking parameters. Achieve online monitoring and elimination of air holes.
Effective closure of pores within 50μm is achieved, the improvement of part surface roughness and residual pores is improved, real-time monitoring and regulation of porosity per layer is ensured, and the quality and accuracy of additive manufacturing are improved.
Smart Images

Figure CN119035574A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of metal additive manufacturing, and in particular to an online monitoring feedback method and system for pores in a laser powder bed melting additive manufacturing process. Background Art
[0002] Laser Powder Bed Fusion (LPBF) is an important branch of metal additive manufacturing. Its principle is that the laser acts on the powder material, and the scanning path is scanned point by point, line by line / layer by layer to achieve part forming. It is well known that the LPBF process has inherent limitations, including severe porosity, rough surface, large tensile stress, etc. Porosity not only affects the molten pool dynamics, but also significantly affects the mechanical properties of LPBF formed parts. Porosity is a typical pore defect. There are two typical pores inside the LPBF part, namely pores and unfused. When the gas is retained in the molten pool and does not escape in time, tiny pores will be formed inside the component. Most of the pores are round. Unfused is caused by the deviation of process parameters from the optimal melting conditions. For example, when too much powder is melted and the laser energy is insufficient, it will lead to insufficient melting and poor interlayer bonding ability. It is reported that many nickel-based alloy components are prone to pores during the manufacturing process, such as In625, In738LC and Hastelloy X. At present, in experimental research and production practice, in order to control the internal porosity of components, the method of optimizing the manufacturing parameter process is generally adopted, but even so, the porosity cannot be completely eliminated.
[0003] The existing technology for suppressing metallurgical defects in laser powder bed fusion additive manufacturing components mainly uses offline detection combined with process optimization and control, but this consumes a lot of time and resources and cannot guarantee the quality of each part. Although some progress has been made in the online monitoring of pores in additively manufactured components, the elimination of internal pore defects still remains at the process parameters, and there is a lack of a technology that can monitor pore defects online and then close them. Summary of the invention
[0004] The purpose of the present invention is to provide a method and system for online monitoring and feedback of pores in a laser powder bed fusion additive manufacturing process, so as to realize online monitoring of pores in a laser powder bed fusion additive manufacturing process and eliminate them by introducing laser shock peening means.
[0005] According to one aspect of the embodiment, a method for online monitoring and closing of pores in laser powder bed fusion additive manufacturing is proposed, comprising: during the laser powder bed fusion additive manufacturing process, after a layer is processed, the pore defect characteristics of the layer are collected, and the pore defect characteristics are compared with a pore evaluation system. If the pore defect characteristics are lower than a threshold, the next layer is processed; if the pore defect characteristics exceed the threshold, the pores are impacted by in-situ laser until the pore defect characteristics are lower than the threshold.
[0006] In some examples, an electromagnetic eddy current monitoring probe is used to scan the layer to obtain an eddy current image.
[0007] In some examples, a Unet++ network with an attention mechanism is used to extract defect features from eddy current images.
[0008] In some examples, the porosity defect feature includes a porosity defect category, geometric information, and porosity.
[0009] In some examples, the in-situ laser shock parameters include: laser power density of 3.8-4.2 GW / cm 2 , the spot diameter is 0.8-1.2mm, the pulse width is 4-6ns, the spot overlap rate is 45-50%, and the incident angle is 0°.
[0010] In some examples, in-situ laser shocking of pores closes pores within a depth of 50 μm.
[0011] In some examples, the pore evaluation system includes mapping of pore size, location, and porosity to tensile strength and elongation.
[0012] In some examples, after the pores within a depth of 50 μm are closed, in-situ laser remelting is used to improve the surface roughness and residual pores of the layer.
[0013] In some examples, process parameters of the in-situ laser remelting include: a scanning strategy with a rotation angle of 67°, a laser power of 130-160 W, and a scanning speed of 1500-2500 mm / s.
[0014] According to the second aspect of the embodiment, a laser powder bed fusion additive manufacturing pore online monitoring and closing system is proposed, and the laser powder bed fusion additive manufacturing pore online monitoring and closing method is adopted to monitor and eliminate metal pores layer by layer.
[0015] The present invention uses electromagnetic eddy currents to collect images in real time and sends them to an industrial computer. The industrial computer calculates the pore diameter, aspect ratio and porosity based on the eddy current signal, compares the threshold of the evaluation system, controls the laser processing based on the feedback results, or turns on the pore warning, controls the laser and the impact device for regulation. The detection method of this method is intuitive and flexible, and can be used to monitor and regulate the porosity of each layer in real time. The method of the present invention effectively solves the problem that laser powder bed fusion additive manufacturing is difficult to solve, such as insufficient laser energy or gas entering the molten pool causing pore defects. The detection process is intuitive and flexible, and the information is rich, which lays a solid foundation for improving the quality and precision of laser powder bed fusion additive manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1It is a schematic diagram of a laser powder bed fusion additive manufacturing system provided by one embodiment of the present invention.
[0017] Figure 2 It is a flow chart of a method for online monitoring and closing pores in laser powder bed fusion additive manufacturing provided by one embodiment of the present invention.
[0018] Figure 3 It is a schematic diagram of the improved Unet++ network structure incorporating an attention mechanism provided by an embodiment of the present invention. DETAILED DESCRIPTION
[0019] like Figure 1 As shown, a laser powder bed fusion additive manufacturing device includes: a workbench 1, a forming device 2, a guide rail 3, a cavity 4, a galvanometer system 5, a filter device 6, a laser beam 7, a powder spreading device 8, a laser 10, a powder feeding device 13 and an industrial computer.
[0020] The present invention proposes an online pore monitoring and closing system based on the laser powder bed fusion additive manufacturing equipment, the purpose of which is to obtain high-density and high-performance additive manufacturing parts. The system includes: an electromagnetic eddy current monitoring probe 12 and its fixture 11, and a laser impact device 9. Figure 2 As shown, first, the metal powder is fused layer by layer using laser powder bed fusion technology. After one layer is manufactured, the electromagnetic eddy current monitoring probe 12 is used to scan the layer to obtain an eddy current image; the improved Unet++ network with an attention mechanism is used to extract defect features from the eddy current image (including pore defect categories, geometric information, and porosity extraction); the defect features are compared with the evaluation system. If the defect features are not allowed by the evaluation system, the laser impact device 9 emits a laser beam 7, which is modulated by the galvanometer system 5 and irradiated to the defect position. The defect is laser impact strengthened to eliminate it, or the layer is remelted. The present invention achieves closure of pores within 50μm in depth. Laser remelting is used to improve the surface roughness caused by impact strengthening. The present invention ensures that the equipment can spread powder normally.
[0021] Based on Maxwell's theory, magnetic field simulation is performed to design a highly sensitive electromagnetic eddy current monitoring probe 12. Rectangular, cube, and circular array probes are set to monitor component defects. The defect monitoring accuracy and penetration depth are analyzed to determine the final probe structure and achieve a detection resolution of ≤90μm. The monitoring time of the electromagnetic eddy current monitoring probe 12 is less than 0.2s / 100mm 2 , moving speed 50mm / s.
[0022] A large number of pore and tensile strength experiments under different process parameters were prepared. Among them, laser power, scanning speed, scanning spacing, layer thickness, and forming angle were used as manufacturing inputs, CT experiments and mechanical properties tensile experiments were used to analyze the mapping relationship between pore size, position, content and tensile properties, match pore size with tensile strength and elongation data, establish a numerical model of defects and tensile properties, and finally determine the pore quality evaluation system.
[0023] Reference Figure 3 , an improved Unet++ (hereinafter referred to as Unet++) network with an attention mechanism is used to process eddy current images. The improvement is specifically to add an attention mechanism to the encoder of the Unet++ network. The Unet++ network includes a feature extraction structure, a feature classification structure, a decoder, a jump connection structure, and a segmentation extraction structure. The eddy current image collected by the electromagnetic eddy current monitoring probe 12 is converted into a C-scan image, and the defect features are segmented and extracted from the C-scan image using the Unet++ network. The defect features include the location, morphology, and size of the defect. Training of the Unet++ network: a data set is made using the C-scan image, for example, the data set is greater than 10,000 images; to ensure the stability of the data, the location, morphology, and size of the defect in the C-scan image are annotated, and a training set and a test set are established. The Unet++ network is trained using the training set images, and then the verification set images are used to verify the effect of the trained Unet++ network segmentation and extraction of defect features. The improved Unet++ network with an attention mechanism can realize the rapid identification and segmentation of pore information in complex environments, and improve the accuracy, processing time, and anti-interference ability of image segmentation. The signal processing time for online defect monitoring is ≤200ms. The segmentation accuracy can reach over 95%.
[0024] In addition, in order to ensure the accuracy of electromagnetic eddy current monitoring, CT detection is used to verify the eddy current monitoring results to ensure the reliability of the data.
[0025] As described above, the present invention provides an online monitoring system for pores in the laser powder bed fusion additive manufacturing process. By collecting and processing the defects in the solidification layer and the impact layer, the position and geometric information of metallurgical defects such as pores, unfusion, and cracks in the manufacturing process are extracted, and the defect position information is provided for the online control of laser shock strengthening.
[0026] The following is an application case.
[0027] First, use 3D software to model parts, slice the model and plan the path, the slice thickness is 35-60μm, and the scanning path is orthogonal scanning. Secondly, select metal powder with good fluidity (such as GH3536 metal powder) for selection, the powder particle size is required to be 0-53μm, and select the best forming parameters of the alloy: laser power is 260-300W, scanning speed is 1000-1500mm / s, scanning spacing is 60-80μm, layer thickness is 35-60μm, substrate is preheated to 100℃, argon protection; then, vacuum the molding chamber and preheat the substrate; finally, print layer by layer.
[0028] Each time a layer is printed, a circular array of electromagnetic eddy current monitoring probes 12 is used to scan the layer back and forth, realizing large-scale, multi-angle defect rapid collection. The defect monitoring accuracy can reach 10μm.
[0029] An improved Unet++ network with attention mechanism is used to extract defect features from eddy current images.
[0030] In-situ laser impact pores. The evaluation system is used to evaluate the pore quality in real time. If the pore index is higher than the threshold, the in-situ laser impacts the pores again until the pores are closed, for example, the pores are closed within 50μm in depth. For example, the in-situ laser impact parameters include: laser power density of 4GW / cm 2 , the spot diameter is 1mm, the pulse width is 5ns, the spot overlap rate is 50%, and the incident angle is 0°.
[0031] In-situ laser remelting improves surface roughness and residual pores. In order to avoid problems such as poor powder spreading effect caused by surface roughness caused by laser impact, in-situ laser remelting is used to improve surface quality, and the limited processing depth reaches 100μm. At the same time, residual pores on the surface and sub-surface of the component are eliminated. The process parameters of in-situ laser remelting take into account the relationship between alloy and energy density output, ensure surface roughness and avoid cracks. A 67° rotating scanning strategy is used, the laser power is 150W, and the scanning speed is 2000mm / s.
Claims
1. A method for online monitoring and closing of pores in laser powder bed fusion additive manufacturing, characterized in that: include: During the laser powder bed fusion additive manufacturing process, after one layer is processed, the pore defect characteristics of the layer are collected and compared with the pore evaluation system. If the pore defect characteristics are lower than the threshold, the next layer is processed. If the pore defect characteristics exceed the threshold, in-situ laser impact is used to shock the pores until the pore defect characteristics are lower than the threshold.
2. The method for online monitoring and closing pores in laser powder bed fusion additive manufacturing according to claim 1, characterized in that: The layer is scanned by an electromagnetic eddy current monitoring probe to obtain an eddy current image.
3. The method for online monitoring and closing pores in laser powder bed fusion additive manufacturing according to claim 2, characterized in that: The Unet++ network with attention mechanism is used to extract defect features from eddy current images.
4. The method for online monitoring and closing pores in laser powder bed fusion additive manufacturing according to claim 1, characterized in that: The pore defect features include pore defect type, geometry information, and porosity.
5. The method for online monitoring and closing pores in laser powder bed fusion additive manufacturing according to claim 1, characterized in that: In-situ laser shock parameters include: laser power density of 3.8-4.2GW / cm 2 , the spot diameter is 0.8-1.2mm, the pulse width is 4-6ns, the spot overlap rate is 45-50%, and the incident angle is 0°.
6. The method for online monitoring and closing pores in laser powder bed fusion additive manufacturing according to claim 5, characterized in that: In-situ laser shock pores close the pores within 50μm in depth.
7. The method for online monitoring and closing pores in laser powder bed fusion additive manufacturing according to claim 1, characterized in that: The pore evaluation system includes the mapping relationship between pore size, location, porosity, tensile strength and elongation.
8. The method for online monitoring and closing pores in laser powder bed fusion additive manufacturing according to claim 5, characterized in that: After the pores within 50 μm in depth were closed, in-situ laser remelting was used to improve the surface roughness and residual pores of the layer.
9. The method for online monitoring and closing pores in laser powder bed fusion additive manufacturing according to claim 8, characterized in that: The process parameters of in-situ laser remelting include: scanning strategy with a rotation angle of 67°, laser power of 130-160W, and scanning speed of 1500-2500mm / s.
10. A laser powder bed fusion additive manufacturing pore online monitoring and closing system, characterized in that: The laser powder bed melting additive manufacturing pore online monitoring and closing method described in any one of claims 1 to 9 is used to monitor and eliminate metal pores layer by layer.
Citation Information
Cited By
Eddy current online monitoring device and method for laser powder bed melting additive manufacturing
CN119952087A