Brazing method of TiCo brazing filler metal for ultra-high-temperature service TiAl alloy brazing component
By using TiCo solder, the problem that the existing solder is unable to maintain the mechanical properties of TiAl alloy joints at high temperatures is solved, and high-temperature service performance is achieved above 900℃ and has excellent room temperature and high-temperature mechanical properties.
Patent Information
- Application Number
- CN202411316312.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-29
AI Technical Summary
The existing solder is unable to maintain the mechanical properties of TiAl alloy joints at a service temperature above 900°C, and it is difficult to meet the requirements of high-temperature service.
TiCo solder is used to melt at atomic percentage of 45% to 50% Co and the remaining Ti to prepare TiCo solder sheets, and then insulated at 1350℃ to 1450℃ for 5 minutes to 25 minutes through vacuum brazing technology to form high melting Brazed joints at temperature.
TiCo solder has good wetting properties and high melting temperature, ensuring excellent mechanical properties of the brazed joint at room temperature and high temperature. The room temperature shear strength reaches more than 390MPa, and the high temperature shear strength of 950℃ is ≥280MPa.
Smart Images

Figure CN119035687A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of brazing. Background Art
[0002] TiAl intermetallic compounds have low density (3.7-3.9 g / cm 3 ), and has high specific elastic modulus and strength, especially at high temperatures above 850°C, it can still maintain sufficient strength, has excellent oxidation resistance and creep resistance, and has great application prospects in the aerospace field. For example, the use of TiAl intermetallic compounds instead of nickel-based high-temperature alloys in rocket engines can greatly reduce the mass of the thrust chamber, thereby improving the overall load capacity of the rocket.
[0003] TiAl alloy has poor plasticity at room temperature and is difficult to process and form. In order to promote the application of TiAl alloy in aerospace engineering, the connection problem of TiAl alloy itself must be solved first. At present, the main connection methods of TiAl alloy are diffusion welding, fusion welding and brazing. Among them, fusion welding has a fast cooling speed and uneven temperature field, which will cause large thermal stress, resulting in cracks in the joint, which greatly reduces the mechanical properties of the joint; although diffusion welding can achieve the connection of TiAl alloy, its connection process is complicated and has strict requirements on the connection interface, which is not conducive to large-scale promotion. Using brazing to connect TiAl alloy is simple to operate, has high joint strength and strong adaptability, and is an important method to promote the application of TiAl alloy.
[0004] At present, the commonly used solders for TiAl alloys mainly include Ag solder, Ti-based solder and Cu-Ti-Ni-Zr series amorphous solders, among which Ag-based solder and amorphous solder usually have good wettability with TiAl alloy parent materials and can obtain reliable joints at room temperature. However, due to the low liquidus line of the solder itself, the obtained TiAl alloy brazed components will fail at temperatures above 500°C, which is difficult to meet the high-temperature service requirements of TiAl alloys in aerospace such as hypersonic aircraft. Ti-based solders have a relatively high melting point. The room temperature strength of the commonly used Ti-based solders when connecting TiAl alloys can reach more than 300MPa, but the shear strength at high temperature is greatly reduced compared to room temperature, and the high-temperature performance needs to be improved urgently. Therefore, it is urgent to develop a solder and a brazing method that can maintain the mechanical properties of TiAl alloy joints at high temperatures, especially at service temperatures above 900°C. Summary of the invention
[0005] The present invention aims to solve the problem that the existing brazing filler metal brazed TiAl alloy brazed components cannot maintain the mechanical properties of the TiAl alloy joints at a service temperature above 900°C, and further provides a brazing method for ultra-high temperature service TiAl alloy brazed components using TiCo filler metal.
[0006] A brazing method for a TiCo brazing filler metal used for a TiAl alloy brazing component in ultra-high temperature service is carried out according to the following steps:
[0007] 1. Weighing a raw material according to 45% to 50% atomic percentage of Co and the balance of Ti to obtain a weighed raw material;
[0008] 2. Melting the weighed raw materials to obtain alloy ingots;
[0009] 3. Slice the alloy ingot into thin slices, grind and polish them to obtain TiCo brazing filler metal slices;
[0010] 4. Stack TiAl alloy, TiCo brazing filler metal sheet and TiAl alloy in order to obtain components to be welded, put the components to be welded into a vacuum brazing furnace and evacuate, then keep the temperature at 1350℃~1450℃ for 5min~25min, cool to 200~500℃ after keeping, then cool to room temperature with the furnace, and finally take out the sample, thus completing the brazing method of TiCo brazing filler metal for ultra-high temperature service TiAl alloy brazing components.
[0011] The beneficial effects of the present invention are:
[0012] 1. The TiCo solder in the present invention has good wettability with the base material. Ti in the solder is a constituent element of the TiAl alloy, and Co is a commonly used element for regulating the composition of the TiAl alloy, and has good compatibility, so the solder has good wettability with the base material. After welding, Co in the solder and the base material form a good mutual diffusion, and a uniform continuous phase structure is formed on both sides. At the same time, Ti and Co elements are both common metal elements, the solder production cost is low, and there is a promising application prospect.
[0013] Second, the solder used in the present invention has a relatively high melting point, and the liquidus temperature is between 1300°C and 1325°C, which can ensure the high temperature resistance of the brazed joint.
[0014] 3. The TiCo solder of the present invention is kept at a brazing temperature of 1450°C for 10 minutes, and the average shear strength of the joint obtained at room temperature reaches more than 390MPa, and the average shear strength at high temperature of 950°C is ≥280MPa, and it has excellent room temperature and high temperature mechanical properties.
[0015] Instruction Manual
[0016] Figure 1 This is a microstructure morphology of the TiCo solder sheet prepared in step 3 of Example 1;
[0017] Figure 2 The room temperature and high temperature shear strength diagram of the joint of the TiAl alloy brazing component prepared in Example 1;
[0018] Figure 3The morphology of the brazed joint and the element surface scanning analysis diagram of the TiAl alloy brazed component prepared in Example 1. DETAILED DESCRIPTION
[0019] Specific implementation method 1: This implementation method is a brazing method for ultra-high temperature service TiAl alloy brazing components using TiCo brazing filler metal, which is carried out according to the following steps:
[0020] 1. Weighing a raw material according to 45% to 50% atomic percentage of Co and the balance of Ti to obtain a weighed raw material;
[0021] 2. Melting the weighed raw materials to obtain alloy ingots;
[0022] 3. Slice the alloy ingot into thin slices, grind and polish them to obtain TiCo brazing filler metal slices;
[0023] 4. Stack TiAl alloy, TiCo brazing filler metal sheet and TiAl alloy in order to obtain components to be welded, put the components to be welded into a vacuum brazing furnace and evacuate, then keep the temperature at 1350℃~1450℃ for 5min~25min, cool to 200~500℃ after keeping, then cool to room temperature with the furnace, and finally take out the sample, thus completing the brazing method of TiCo brazing filler metal for ultra-high temperature service TiAl alloy brazing components.
[0024] The beneficial effects of this embodiment are:
[0025] 1. The TiCo solder in this embodiment has good wettability with the base material. Ti in the solder is a constituent element of the TiAl alloy, and Co is a commonly used element for regulating the composition of the TiAl alloy, and has good compatibility, so the solder has good wettability with the base material. After welding, Co in the solder and the base material form a good mutual diffusion, and a uniform continuous phase structure is formed on both sides. At the same time, Ti and Co elements are both common metal elements, and the solder production cost is low, which has application prospects.
[0026] 2. The solder used in this embodiment has a relatively high melting point, and the liquidus temperature is between 1300°C and 1325°C, which can ensure the high temperature resistance of the brazed joint.
[0027] 3. The TiCo brazing filler metal described in this embodiment is kept at a brazing temperature of 1450°C for 10 minutes, and the obtained joint has an average shear strength of more than 390MPa at room temperature and an average shear strength of ≥280MPa at 950°C, and has excellent room temperature and high temperature mechanical properties.
[0028] Specific embodiment 2: This embodiment differs from the specific embodiment 1 in that: in step 1, TiH is weighed according to 45% to 50% Co and the remainder Ti by atomic percentage. 2Powder and Co powder. Others are the same as those in the first embodiment.
[0029] Specific implementation method 3: This implementation method is different from specific implementation methods 1 or 2 in that: in step 2, the weighed raw materials are placed in a vacuum arc melting furnace for melting and turned over multiple times under a vacuum environment or an argon atmosphere. The rest is the same as specific implementation methods 1 or 2.
[0030] Specific embodiment 4: This embodiment is different from specific embodiments 1 to 3 in that the thickness of the TiCo solder sheet in step 3 is 200 μm to 300 μm. Other aspects are the same as specific embodiments 1 to 3.
[0031] Specific embodiment 5: This embodiment is different from specific embodiments 1 to 4 in that the TiAl alloy described in step 4 is Ti-48Al, Ti-42Al-5V, Ti-45Al-8.5Nb-0.2W-0.03Y or Ti-48Al-2Cr-2Nb. The rest is the same as specific embodiments 1 to 4.
[0032] Specific embodiment 6: This embodiment is different from specific embodiments 1 to 5 in that the TiAl alloy described in step 4 is a pre-treated TiAl alloy; the pre-treatment specifically includes sanding with sandpaper to remove the surface oxide layer of the TiAl alloy, and then ultrasonic cleaning in acetone. The rest is the same as specific embodiments 1 to 5.
[0033] Specific embodiment 7: This embodiment is different from specific embodiments 1 to 6 in that the TiCo solder flakes in step 4 are pre-treated TiCo solder flakes; the pre-treatment is ultrasonic cleaning in acetone. The rest is the same as specific embodiments 1 to 6.
[0034] Specific embodiment 8: This embodiment differs from any one of specific embodiments 1 to 7 in that: in step 4, the component to be welded is placed in a vacuum brazing furnace and evacuated to 5×10 -3 Pa or less. The rest is the same as the first to seventh embodiments.
[0035] Specific embodiment 9: This embodiment is different from specific embodiments 1 to 8 in that: in step 4, the temperature is first heated to 100°C at a rate of 5°C / min to 20°C / min, then heated to 1000°C at a rate of 10°C / min to 15°C / min, and finally heated to 1350°C to 1450°C at a rate of 5°C / min to 10°C / min. The rest is the same as specific embodiments 1 to 8.
[0036] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that: in step 4, the temperature is lowered to 200° C. to 500° C. at a rate of 5° C. / min to 10° C. / min. The rest is the same as specific embodiments 1 to 9.
[0037] The following examples are used to verify the beneficial effects of the present invention:
[0038] Embodiment 1:
[0039] A brazing method for a TiCo brazing filler metal used for a TiAl alloy brazing component in ultra-high temperature service is carried out according to the following steps:
[0040] 1. Weigh TiH with 50% Co and the remainder Ti as atomic percentage 2 powder and Co powder to obtain the weighed raw material;
[0041] 2. Under an argon atmosphere, the weighed raw materials are placed in a vacuum arc melting furnace for melting and turned over several times to obtain an alloy ingot;
[0042] 3. Slice the alloy ingot into thin slices, grind and polish them to obtain TiCo brazing filler metal slices;
[0043] 4. Stack the TiAl alloy, TiCo brazing filler metal sheet and TiAl alloy in the order to obtain the components to be welded. Put the components to be welded into a vacuum brazing furnace and evacuate to 5×10 -3 Pa, and then heated to 100°C at a rate of 5°C / min, then heated to 1000°C at a rate of 15°C / min, and finally heated to 1450°C at a rate of 10°C / min, and kept warm at 1450°C for 10 minutes. After keeping warm, the temperature was lowered to 400°C at a rate of 8°C / min, and then cooled to room temperature with the furnace, and finally the sample was taken out to obtain a TiAl alloy brazing component, that is, the brazing method of TiCo brazing filler metal for ultra-high temperature service TiAl alloy brazing components was completed.
[0044] The thickness of the TiCo solder sheet described in step 3 is 250 μm.
[0045] The TiAl alloy described in step 4 is Ti-42Al-5V.
[0046] The TiAl alloy described in step 4 is a pretreated TiAl alloy; the pretreatment specifically comprises polishing with sandpaper to remove the oxide layer on the surface of the TiAl alloy, and then ultrasonically cleaning it in acetone for 10 minutes.
[0047] The TiCo solder sheet described in step 4 is a pretreated TiCo solder sheet; the pretreatment is specifically ultrasonic cleaning in acetone for 10 minutes.
[0048] Figure 1 This is a microstructure morphology of the TiCo solder sheet prepared in step 3 of Example 1. As can be seen from the figure, a uniform intermetallic compound structure is formed after arc melting, and no other phases exist in the solder.
[0049] According to the national standard GB / T 11363-2008, the shear strength of the TiAl alloy brazing component prepared in Example 1 was tested; Figure 2 The figure shows the room temperature and high temperature shear strength of the joint of the TiAl alloy brazed component prepared in Example 1. As can be seen from the figure, the TiCo brazing filler metal of this example can achieve high-quality connection of the TiAl alloy, with an average room temperature shear strength of 392 MPa and an average high temperature shear strength of 280 MPa at 950°C, which effectively improves the room temperature and high temperature mechanical properties of the TiAl alloy and greatly improves the service temperature of the TiAl alloy brazed component.
[0050] Figure 3 The brazed joint morphology and element surface scanning analysis diagram of the TiAl alloy brazed component prepared in Example 1; it can be seen from the figure that Co in the brazing material and the base material form a good mutual diffusion, a uniform continuous phase structure is formed on both sides, and the brazing seam width is only about 1 micron, which greatly avoids the formation of brittle phase and improves the service temperature of the joint and the stability under service conditions.
Claims
1. A brazing method for TiCo brazing filler metal for ultra-high temperature service TiAl alloy brazing components, characterized in that It is carried out in the following steps:
1. Weighing a raw material according to 45% to 50% atomic percentage of Co and the balance of Ti to obtain a weighed raw material; 2. Melting the weighed raw materials to obtain alloy ingots; 3. Slice the alloy ingot into thin slices, grind and polish them to obtain TiCo brazing filler metal slices; 4. Stack TiAl alloy, TiCo brazing filler metal sheet and TiAl alloy in order to obtain components to be welded, put the components to be welded into a vacuum brazing furnace and evacuate, then keep the temperature at 1350℃~1450℃ for 5min~25min, cool to 200~500℃ after keeping, then cool to room temperature with the furnace, and finally take out the sample, thus completing the brazing method of TiCo brazing filler metal for ultra-high temperature service TiAl alloy brazing components.
2. The brazing method of a TiCo brazing filler metal for ultra-high temperature service TiAl alloy brazing components according to claim 1, characterized in that In step 1, TiH2 powder and Co powder are weighed according to the atomic percentage of 45% to 50% Co and the balance Ti.
3. The brazing method of a TiCo brazing filler metal for ultra-high temperature service TiAl alloy brazing components according to claim 1, characterized in that In step 2, the weighed raw materials are placed in a vacuum arc melting furnace for melting and turned over several times under a vacuum environment or an argon atmosphere.
4. The brazing method of a TiCo brazing filler metal for ultra-high temperature service TiAl alloy brazing components according to claim 1, characterized in that The thickness of the TiCo solder sheet described in step 3 is 200 μm to 300 μm.
5. The brazing method of TiCo brazing filler metal for ultra-high temperature service TiAl alloy brazing components according to claim 1, characterized in that The TiAl alloy described in step 4 is Ti-48Al, Ti-42Al-5V, Ti-45Al-8.5Nb-0.2W-0.03Y or Ti-48Al-2Cr-2Nb.
6. The brazing method of TiCo brazing filler metal for ultra-high temperature service TiAl alloy brazing components according to claim 1, characterized in that The TiAl alloy described in step 4 is a pretreated TiAl alloy; the pretreatment specifically comprises polishing with sandpaper to remove the oxide layer on the surface of the TiAl alloy, and then ultrasonically cleaning it in acetone.
7. The brazing method of a TiCo brazing filler metal for ultra-high temperature service TiAl alloy brazing components according to claim 1, characterized in that The TiCo solder sheet described in step 4 is a pre-treated TiCo solder sheet; the pre-treatment is specifically ultrasonic cleaning in acetone.
8. The brazing method of TiCo brazing filler metal for ultra-high temperature service TiAl alloy brazing components according to claim 1, characterized in that In step 4, the components to be welded are placed in a vacuum brazing furnace and evacuated to 5×10 -3 Below Pa.
9. The brazing method of TiCo brazing filler metal for ultra-high temperature service TiAl alloy brazing components according to claim 1, characterized in that In step 4, the temperature is first heated to 100°C at a rate of 5°C / min to 20°C / min, then heated to 1000°C at a rate of 10°C / min to 15°C / min, and finally heated to 1350°C to 1450°C at a rate of 5°C / min to 10°C / min.
10. The brazing method of TiCo brazing filler metal for ultra-high temperature service TiAl alloy brazing components according to claim 1, characterized in that In step 4, the temperature is lowered to 200°C to 500°C at a rate of 5°C / min to 10°C / min.