Titanium alloy casting laser welding concentric wire feeding protection device and precision repair method

Through the concentric wire feeding protection device of titanium alloy casting laser welding, the protective gas and side blowing gas are used to remove negative substances generated during welding, which solves the problem of difficulty in controlling energy and welding wire melting efficiency in laser welding, and achieves uniform welds Improved performance and mechanical properties.

CN119035763AInactive Publication Date: 2024-11-29CHINA SHIPBUILDING INDUSTRY CORPORATION NO725 RESEARCH INSTITUTE

Patent Information

Application Number
CN202411534588.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-31
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, laser welding of titanium alloys cannot effectively protect lasers, welding wires, droplets, and welds, resulting in the incoming energy and welding wire melting efficiency that cannot be accurately controlled, and columnar dendrite structure is easily formed, affecting the structure and mechanical properties of the welds. Uniformity.

Method used

A concentric wire feeding protection device for laser welding of titanium alloy castings is designed, including a protective cover shell, a hole-shaped conical plate and a plasma suppression device. By protecting the gas and side-blowing gas input, the welding area is protected and the generated during the welding process is removed. Negative substances achieve precise control of energy and weld accuracy.

Benefits of technology

Effectively protect lasers and welding wires, avoid the formation of columnar dendrite structure, improve the uniformity of the structure and mechanical properties of the welds, reduce welding thermal stress and deformation, and meet the welding requirements of precision castings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035763A_ABST
    Figure CN119035763A_ABST
Patent Text Reader

Abstract

The invention relates to the field of metal material welding, and provides a titanium alloy casting laser welding concentric wire feeding protection device and a precision repair method.The protection device comprises a protection cover shell, a conical plate with holes and a plasma suppression device, and a hollow first cavity is defined between the protection cover shell and the conical plate with the holes; a second cavity with an upper opening and a lower opening is defined by the perforated conical plate, a protective gas inlet pipe is arranged on the protective cover shell and used for conveying protective gas into the first cavity, a perforated bottom plate is arranged at the bottom of the first cavity, and a plurality of second gas holes are formed in the perforated conical plate and used for guiding the protective gas in the first cavity into the second cavity. And the plasma suppression device penetrates through the second cavity and is used for blowing away negative substances during laser welding. Through the arrangement of the protection device, laser, welding wires, molten drops and welding seams can be effectively protected, negative substances such as plasmas on the surface of a molten pool can be removed, and the uniformity of the welding seam structure and the mechanical property is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal material welding, and in particular to a concentric wire feeding protection device for laser welding of titanium alloy castings and a precision repair method. Background Art

[0002] CB 20030-2011 "Technology Requirements for Repair Welding of Titanium and Titanium Alloy Castings for Ships" and HB / Z 348-2001 "Technology and Inspection of Repair Welding of Titanium Alloy Castings" standards stipulate that the repair welding method for titanium alloy castings is manual tungsten inert gas welding, which is simple and convenient to operate. However, manual tungsten inert gas welding has a large welding heat input and large welding deformation, which will cause precision titanium alloy castings with high dimensional accuracy requirements to be out of tolerance and unqualified. Therefore, there is a strong demand for low heat input and high precision repair welding methods for titanium alloy precision castings in the industry.

[0003] CN201710647219.4 discloses a method for precision laser repair welding of defects in titanium alloy parts. Through welding preparation processing groove, electron beam repair welding and post-weld treatment, it can solve the problems of welding defects such as unfusion, pores and inclusions in the weld after welding of thick titanium alloys, such as long repair cycle, large processing size, large repair workload, large welding deformation, poor stability of organizational properties, etc., reduce repair costs, improve repair efficiency, and at the same time, it can repair defects such as pits and cracks that appear during the processing and use of precision parts, solve the problem that conventional welding methods for repairing defects of precision parts cannot meet the requirements, achieve precision repair, avoid the generation of scrapped parts, and reduce use costs. This patent uses laser welding to repair titanium alloy parts. Although it can change the problem of large welding deformation to a certain extent, it cannot provide perfect protection for the laser, welding wire, molten droplet and weld during the welding process, resulting in the inability to accurately control the input energy, welding wire melting efficiency and weld accuracy. In addition, the above-mentioned structure comes into contact with the air or negative substances generated during welding, which easily forms a columnar dendrite structure in the weld, seriously affecting the uniformity of the structure and mechanical properties of the repair weld. Summary of the invention

[0004] The problem to be solved by the present invention is that, in the prior art, the laser welding method is used for titanium alloy repair welding. Although it can change the problem of large welding deformation to a certain extent, it is impossible to perfectly protect the laser, welding wire, molten droplet and weld during the welding process, resulting in the inability to accurately control the input energy, welding wire melting efficiency and weld accuracy, and it is easy to form a columnar dendrite structure in the weld, which seriously affects the uniformity of the structure and mechanical properties of the repair weld.

[0005] The invention discloses a concentric wire feeding protection device for laser welding of titanium alloy castings, comprising a protective cover shell, a perforated conical plate and a plasma suppression device, wherein a hollow first chamber is enclosed between the protective cover shell and the perforated conical plate, the perforated conical plate is arranged on the inner side of the protective cover shell, the perforated conical plate is enclosed to form a second chamber with upper and lower openings, the second chamber is a frustum-shaped chamber which gradually shrinks from top to bottom, during laser welding, a laser beam and a welding wire coaxially pass through the second chamber for welding, a protective air inlet pipe is arranged on the protective cover shell, the protective air inlet pipe is used to transport protective gas into the first chamber, a perforated bottom plate is arranged at the bottom of the first chamber, a plurality of first air holes are arranged on the perforated bottom plate, a plurality of second air holes are arranged on the perforated conical plate, the second air holes connect the first chamber with the second chamber, and are used to introduce the protective gas in the first chamber into the second chamber, the plasma suppression device is arranged through the second chamber, and is used to blow away negative substances around the molten droplets formed by melting of the welding wire during laser welding.

[0006] Furthermore, the plasma suppression device includes a side blowing air inlet pipe and a side blowing pipe, the side blowing pipe is arranged through the second chamber, the first end of the side blowing pipe is connected to the side blowing air inlet pipe, and the second end is arranged near the periphery of the molten droplet of the welding wire during laser welding, the side blowing air inlet pipe is used to transport side blowing gas into the side blowing pipe, and the side blowing pipe is used to use the side blowing gas to blow away negative substances generated during the laser welding process.

[0007] Furthermore, there are more than two side blowing pipes, and the more than two side blowing pipes are evenly distributed around the axial direction of the welding wire.

[0008] Furthermore, a perforated partition is horizontally arranged in the first chamber, and the perforated partition is used to divide the space in the first chamber. A plurality of third air holes are arranged on the perforated partition, and the third air holes are used to connect the space divided by the perforated partition.

[0009] Furthermore, the perforated partitions are provided with 1-3 layers. When more than two layers are provided, the third air holes on adjacent perforated partitions are staggered.

[0010] The present invention also provides a precision repair method for titanium alloy castings, using the titanium alloy casting laser welding concentric wire feeding protection device as described above, the precision repair method comprising: Step S1: Beveling the casting surface at defective locations, and degreasing and cleaning the area to be welded; Step S2: delivering shielding gas from the shielding gas inlet pipe to the first chamber so that the high-temperature area during the laser welding process is within the protection range of the shielding gas, and delivering side-blowing gas to the plasma suppression device to blow away negative substances generated during the laser welding process; Step S3: setting welding parameters and starting laser welding. During the welding process, shielding gas and side blowing gas are continuously input; Step S4: After reaching the welding end position, turn off the laser beam, turn off the side blowing gas, maintain the shielding gas input until the first preset condition is reached, turn off the shielding gas, and end the welding.

[0011] Furthermore, the groove in step S1 is an inverted trapezoidal structure, the groove bottom width a is consistent with the welding spot width, the groove depth C is consistent with the defect depth, transition angles with a radius of R are set on both sides of the groove bottom, and the groove upper end opening width b is greater than a3mm-5mm.

[0012] Furthermore, in step S3, the laser beam used for welding is a concentric pulsed double annular spot, the laser power of the outer annular spot is smaller than the laser power of the inner annular spot, the outer annular spot is used to preheat the base material near the weld, and the inner annular spot is used for laser welding.

[0013] Furthermore, in step S3, the welding parameters include: The laser beam spot is one of the following shapes: circular, rectangular, triangular, elliptical, figure 8, and trapezoidal. The laser power of the outer ring spot is 2000W-4000W, and the laser power of the inner ring spot is 6000W-15000W. The defocus is -10mm-10mm, the wire feeding speed is 0.4m / min-3m / min, the welding speed is 0.6m / min-2.0m / min, and the welding wire is placed in the center of the spot shape.

[0014] Furthermore, the first preset condition in step S4 includes: the temperature of the high temperature area of ​​laser welding is cooled to below 100° C., and / or, after the laser is turned off, the shielding gas is continuously input for more than 30 seconds.

[0015] Compared with the prior art, the titanium alloy casting laser welding concentric wire feeding protection device and precision repair method described in the present invention have the following advantages: The present invention can effectively protect the laser, welding wire, molten droplet and weld during repair welding by setting the protective device, and can also effectively remove negative substances such as plasma on the surface of the molten pool, realize accurate control of input energy, welding wire deposition efficiency and weld accuracy, avoid the formation of columnar dendrite structure in the weld, and improve the uniformity of the structure and mechanical properties of the repair weld. Through the setting of concentric pulse double ring spot, the parent material near the weld can be effectively preheated, the temperature difference between the molten pool and the parent material during welding is reduced, the welding thermal stress and deformation are reduced, and the stability of the molten pool and the crack resistance of the joint are improved. The welding deformation can be within 0.5 mm, which meets the general repair welding requirements of precision castings. The protective device provided by the present invention has a simple structure and is easy to use, and significantly improves the uniformity of the structure and mechanical properties of the repair weld. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 A top view of a concentric wire feeding protection device for laser welding of titanium alloy castings according to an embodiment of the present invention; Figure 2 It is a schematic cross-sectional structure diagram of a concentric wire feeding protection device for laser welding of titanium alloy castings according to an embodiment of the present invention; Figure 3 It is a structural schematic diagram of the groove described in an embodiment of the present invention.

[0017] Description of reference numerals: 1. Side blowing air inlet pipe; 2. Side blowing pipe; 3. Protective cover shell; 4. Conical plate with holes; 5. Laser beam; 6. Welding wire; 7. Protective air inlet pipe; 8. Perforated partition plate; 9. Molten droplet; 10. Negative matter; 11. Welding seam; 12. Casting; 13. Perforated bottom plate. DETAILED DESCRIPTION

[0018] To make the purpose, technical solutions and advantages of the present invention clearer, the present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. The specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0019] A titanium alloy casting laser welding concentric wire feeding protection device and a precision repair method according to an embodiment of the present invention will be described in detail below with reference to the accompanying drawings.

[0020] Example 1

[0021] This embodiment provides a titanium alloy casting laser welding concentric wire feeding protection device, such as Figure 1-Figure 3As shown, it includes a protective cover shell 3, a perforated conical plate 4 and a plasma suppression device. A hollow first chamber is enclosed between the protective cover shell 3 and the perforated conical plate 4. The perforated conical plate 4 is arranged on the inner side of the protective cover shell 3. The perforated conical plate 4 encloses a second chamber with upper and lower openings. The second chamber is a frustum-shaped cavity that gradually shrinks from top to bottom. During laser welding, the laser beam 5 and the welding wire 6 coaxially pass through the second chamber for welding. A protective air inlet pipe 7 is arranged on the protective cover shell 3. The protective air inlet pipe 7 is used to transport protective gas into the first chamber. A perforated bottom plate 13 is arranged at the bottom of the first chamber. A plurality of first air holes are arranged on the perforated bottom plate 13. A plurality of second air holes are arranged on the perforated conical plate 4. The second air holes connect the first chamber with the second chamber and are used to introduce the protective gas in the first chamber into the second chamber. The plasma suppression device is arranged through the second chamber and is used to blow away negative substances 10 around the molten droplet 9 formed by the melting of the welding wire 6 during laser welding.

[0022] Among them, the negative substances 10 include one or more of plasma, plume and metal smoke. During the laser welding process, the coaxially fed welding wire 6 melts under the irradiation of the annular laser beam 5 to form a molten droplet 9, and a small amount of vaporization occurs. At this time, negative substances 10 such as plasma, plume and metal smoke are formed. After the plasma is formed, it will reflect, scatter, absorb and other effects on the incident laser beam 5 through refraction and radiation, and will form a shielding effect on the laser beam 5, thereby affecting the coupling of laser energy with the workpiece; and the plasma will reduce the laser power and the concentration of the heat source, which may lead to reduced penetration, pore generation and changes in the structural composition of the weld 11, ultimately affecting the welding quality and the reliability of the process. As the plasma gathers more, its influence on laser welding is also greater, the laser becomes more divergent, the energy density decreases, and the penetration depth is reduced. The plume will absorb, scatter and refract the laser beam 5, resulting in laser energy loss and reduced welding efficiency and quality. In addition, the plume may also affect the stability of the welding process, leading to molten pool fluctuations, spattering and other problems, thereby affecting the formation and quality of the weld 11. The negative impact of metal smoke on laser welding is mainly reflected in the impact on welding quality and working environment. The metal smoke particles generated during laser welding are easy to adhere to the weld 11 or surrounding materials, resulting in welding defects such as pores and inclusions, reducing welding quality and the mechanical strength of the weld 11. In addition, the smoke will pollute the working environment and cause harm to the health of operators. It can be seen that the generation and accumulation of plasma, plume and metal smoke will block the propagation of the laser beam 5 and seriously affect the welding quality. In this embodiment, by setting up a plasma suppression device, negative substances 10 generated during the laser welding process can be blown away in time, ensuring the propagation stability and propagation efficiency of the laser beam 5, which is beneficial to the control of input energy, welding wire melting efficiency and weld 11 accuracy, and significantly improving the uniformity of the organization and mechanical properties of the repair weld 11.In addition, the arrangement of the perforated bottom plate 13 in the first chamber allows a portion of the protective gas in the first chamber to overflow from the first pores, thereby covering the high-temperature weld 11, so that the weld 11 and the high-temperature area near it can be cooled in the atmosphere of the protective gas, thereby avoiding oxidation of the weld 11 and the surrounding area, and preventing impurities such as nitrogen and oxygen from entering the weld 11, and maintaining the temperature of the welding area stable, so that the weld 11 can be cooled evenly, reducing the generation of cooling deformation and cracks, and another portion of the protective gas in the first chamber passes through the second pores of the perforated conical plate 4. Overflow, the second chamber is conical and has upper and lower openings. On the one hand, after the protective gas overflows from the perforated conical plate 4, the gas flow near the smaller opening at the lower end is sufficient and the air pressure is higher. Since the end with the smaller opening is closer to the molten pool, the more sufficient gas flow and higher air pressure can provide better protection for the molten pool. On the other hand, the upper opening is larger, so that most of the protective gas is discharged through the upper opening, which can effectively prevent external air from mixing into the second chamber, ensuring the purity of the protective gas ejected from the lower opening, thereby improving the protection effect during laser welding. Specifically, the number, diameter and air intake of the protective air inlet pipe 7 can be set according to the requirements of the specific process for the protective gas flow, which will not be repeated here.

[0023] In this embodiment, if Figure 1 , Figure 2 As shown, the plasma suppression device includes a side blowing air inlet pipe 1 and a side blowing pipe 2, the side blowing pipe 2 is arranged through the second chamber, the first end of the side blowing pipe 2 is connected to the side blowing air inlet pipe 1, and the second end is arranged near the periphery of the molten droplet 9 of the welding wire 6 during laser welding, the side blowing air inlet pipe 1 is used to transport the side blowing gas into the side blowing pipe 2, and the side blowing pipe 2 is used to use the side blowing gas to blow away the negative substances 10 generated during the laser welding process. The second end of the side blowing pipe 2 is closer to the position where the molten droplet 9 drips, so that the negative substances 10 at the lower end of the molten droplet 9 and the welding wire 6 can be effectively suppressed, the propagation stability and propagation efficiency of the laser beam 5 are ensured, and the welding parameters related to the laser beam 5 can be more accurately controlled, which significantly improves the welding stability and welding quality.

[0024] As an optional embodiment, the side blowing pipes 2 are provided with more than two, and the more than two side blowing pipes 2 are evenly arranged around the axial direction of the laser welding wire 6. This arrangement helps to evenly blow away the negative substances 10 around the molten droplet 9 during welding, improves the blowing effect, and prevents the molten droplet 9 from drifting when the negative substances 10 are blown by the side blowing gas in a single side blowing pipe 2, thereby ensuring the stability of the molten pool, thereby ensuring the uniformity of the structure and mechanical properties of the repair weld 11.

[0025] Preferably, Figure 1As shown, there are three side blowing pipes 2, and the three side blowing pipes 2 are evenly arranged around the axial direction of the welding wire 6. The angle between the three side blowing pipes 2 is 120°. This arrangement can blow away the negative substances 10 around the molten droplet 9 without dead angles, thereby significantly improving the transmission effect of the laser beam 5, thereby improving the welding quality. In addition, the type, ratio, flow rate, etc. of the side blowing gas introduced into the three side blowing pipes 2 can be adjusted relatively independently, with strong adjustability, suitable for different casting 12 structural requirements; it can also be adjusted uniformly, which will not be repeated here.

[0026] In one preferred embodiment, Figure 1 As shown, the side blowing pipe 2 is arranged on the inner side wall of the perforated conical plate 4. This arrangement facilitates the fixed arrangement of the side blowing pipe 2 and also facilitates the formation of a certain angle between the side blowing pipe 2 and the welding wire 6 along the side wall of the second chamber, so that the negative material 10 is blown away laterally to avoid contact with the molten pool, thereby ensuring the stability of the weld 11.

[0027] As one of the preferred embodiments, Figure 2 As shown, a perforated partition plate 8 is also horizontally arranged in the first chamber, and the perforated partition plate 8 is used to divide the space in the first chamber. A plurality of third air holes are arranged on the perforated partition plate 8, and the third air holes are used to connect the space divided by the perforated partition plate 8. It should be understood that the shielding gas entering the first chamber through the shielding air inlet pipe 7 usually has a high speed, which forms turbulence in the first chamber, resulting in different gas pressures, gas flow rates and gas directions at each air hole on the perforated conical plate 4 and the perforated bottom plate 13, and different gas pressures, flow rates and directions overflowing therefrom, thereby forming new turbulence after the overflow, and such turbulence easily draws in air, so that it contacts the weld 11 or the molten drop 9, affecting the welding quality. In the present application, by setting the perforated partition 8, the gas in the first chamber can be rectified, so that the speed of the gas overflowing therethrough is greatly reduced. Except for a certain turbulence near the pores, laminar flow is mainly formed on the lower side of the perforated partition 8. In this case, the protective gas can overflow evenly and smoothly through the first pores or the second pores, which greatly reduces the turbulence caused by the above-mentioned flow and significantly improves the protection effect.

[0028] Preferably, the perforated partitions 8 are provided with 1-3 layers. When more than 2 layers are provided, the third pores on adjacent perforated partitions 8 are staggered. The staggered third pores on adjacent perforated partitions 8 can further eliminate the turbulence intensity when the protective gas overflows, thereby greatly eliminating the turbulence formed when the protective gas overflows while making the protective gas overflow evenly and stably, thereby ensuring the protective effect of the protective gas. The staggered third pores can further enhance the rectification effect between two adjacent layers of perforated partitions 8, thereby effectively enhancing the protective gas of the protective gas. Preferably, the perforated partitions 8 have two layers, and the third pores on the two layers of perforated partitions 8 are staggered. This arrangement can divide the first chamber into three layers, with turbulence in the air intake layer and laminar flow in the remaining two layers, which is conducive to the uniform and stable overflow of the protective gas.

[0029] As one of the optional embodiments, the shielding gas and the side blowing gas are both inert gases, and the inert gas is argon, helium, or a mixture of helium and argon. It should be noted that the components of the shielding gas and the side blowing gas are the same or different, which is specifically determined by the requirements of the casting 12 structure and will not be described in detail here.

[0030] As an embodiment of the present invention, the taper of the frustum-shaped cavity of the second chamber is between 0.5-0.7, preferably 0.6. Through the above arrangement, an effective balance of shielding gas overflow can be achieved. On the one hand, air can be effectively prevented from entering the second chamber from the upper opening of the frustum-shaped cavity. On the other hand, the gas flow and pressure of the lower opening of the second chamber can be ensured to fully protect the molten pool, thereby ensuring the stability of laser welding.

[0031] Optionally, the protective cover shell 3 and the perforated conical plate 4 are both arranged in a ring shape, such as Figure 1 This arrangement, together with the filling method of the coaxial filling wire, can effectively maintain the directionality and consistency of the weld 11.

[0032] Correspondingly, a titanium alloy precision casting laser concentric wire feeding precision repair system including the above-mentioned protection device includes a laser welding system, an image acquisition and processing system and a protection device. The structure of the protection device is as described above. During welding, the protection device is arranged above the casting 12 or the parent material. The laser welding system includes at least a laser generating device and a wire feeding device. The laser generating device is used to emit an editable concentric pulse dual-annular laser spot. The laser power of the outer annular spot is relatively low, which is used to preheat the casting 12 parent material near the weld 11, reduce the temperature difference between the molten pool and the parent material during welding, reduce welding thermal stress and deformation, and at the same time, preheating can also improve the stability of the laser welding molten pool and the crack resistance of the joint; the inner annular spot adopts a larger laser power The welding wire 6 is melted at a high rate, and the wire is fed coaxially in the center of the annular spot. The transition form, size and transition frequency of the center welding wire droplet are accurately controlled by online adjusting parameters such as the spot pulse laser power waveform, size and frequency, so as to realize precise control of welding wire deposition. Due to the presence of the side blow pipe 2, the laser input energy can be accurately adjusted, thereby realizing online control of heat input, welding wire deposition efficiency and weld seam 11 size accuracy. Through precise energy control, welding deformation is effectively controlled. At the same time, the protection device can realize effective protection of welding. According to the different types of defects in the casting 12, different repair welding groove forms can be designed, and finally the defects of the titanium alloy precision casting 12 can be repaired, and the welding deformation can be controlled to within 0.5mm, which meets the general repair welding requirements of the precision casting 12.

[0033] Example 2

[0034] This embodiment provides a precision repair method for a titanium alloy casting, using the titanium alloy casting laser welding concentric wire feeding protection device as described in Example 1.

[0035] The repair method comprises: Step S1: Beveling the casting surface at defective locations, and degreasing and cleaning the area to be welded; Step S2: delivering shielding gas from the shielding gas inlet pipe to the first chamber so that the high-temperature area during the laser welding process is within the protection range of the shielding gas, and delivering side-blowing gas to the plasma suppression device to blow away negative substances generated during the laser welding process; Step S3: setting welding parameters and starting laser welding. During the welding process, shielding gas and side blowing gas are continuously input; Step S4: After reaching the welding end position, turn off the laser beam, turn off the side blowing gas, maintain the shielding gas input until the first preset condition is reached, turn off the shielding gas, and end the welding.

[0036] The above-mentioned repair method can realize rapid repair and molding of titanium alloy precision castings with high repair efficiency. Due to the setting of the protective device, the input energy, welding wire melting efficiency and weld accuracy can be achieved, the welding deformation is small, the formation of columnar dendrite structure is suppressed, and the stability of weld structure and mechanical properties is improved.

[0037] Specifically, Figure 3 As shown, the groove in step S1 is an inverted trapezoidal structure, the groove bottom width a is consistent with the welding spot width, the groove depth C is consistent with the defect depth, transition angles with a radius of R are set on both sides of the groove bottom, and the groove upper end opening width b is greater than a3mm-5mm. Optionally, a is 3mm-6mm, which can ensure that the root of the groove is fully fused, b is 6mm-11mm, C is 1mm-4mm, and R is 1mm-2mm to prevent the defect of unfused sides of the root of the groove during repair welding.

[0038] In step S1, degreasing and cleaning the area to be welded includes: Step S11: pickling to remove oil stains; Step S12: Use a carbide grinding head to clean the area to be welded within 15 mm; Step S13: Wipe the area to be welded with acetone or anhydrous alcohol.

[0039] Among them, the pickling in step S11 is performed on the entire casting to be welded.

[0040] Wherein, the flow rate of the side blowing gas in step S2 is greater than or equal to 25 L / min.

[0041] This flow rate can ensure that most of the negative substances generated during laser welding are blown away; the flow rate of the shielding gas needs to be set according to the actual situation so that the high-temperature areas during the welding process are all protected by the shielding gas. I will not go into details here.

[0042] Among them, Figure 1 As shown, in step S3, the laser beam used for welding is a concentric pulse double annular spot, the laser power of the outer annular spot is less than the laser power of the inner annular spot, the outer annular spot is used to preheat the parent material near the weld, and the inner annular spot is used for laser welding. In this embodiment, by using a laser beam of concentric pulse double annular spots, the outer annular spot can preheat the parent material near the weld, reduce the temperature difference between the molten pool and the parent material during welding, reduce welding thermal stress and deformation, and preheating can also improve the stability of the laser welding molten pool and the crack resistance of the joint; the inner annular spot uses a larger laser power to melt the welding wire, and the wire is coaxially fed in the center of the annular spot to achieve precise repair and welding of titanium alloy castings. The attached Figure 1The dotted line at the center of the middle protection device is the concentric pulse double annular light spot. The larger dotted ring on the outside is the outer annular light spot, and the smaller dotted ring on the inside is the inner annular light spot. The outer annular light spot, the inner annular light spot and the welding wire are coaxially arranged.

[0043] Specifically, in step S3, the welding parameters include: The laser beam spot is one of the shapes of circle, rectangle, triangle, ellipse, figure 8, trapezoid, etc. The laser power of the outer ring spot is 2000W-4000W, the laser power of the inner ring spot is 6000W-15000W, the defocus is -10mm-10mm (negative 10mm to 10mm), the wire feeding speed is 0.4m / min-3m / min, the welding speed is 0.6m / min-2.0m / min, and the welding wire is placed in the center of the spot shape.

[0044] It should be noted that the waveform, size, frequency and other parameters of the spot pulse laser in the welding process are all adjustable online. By adjusting the spot pulse laser power waveform, size, frequency and other parameters online, the transition form, size and transition frequency of the central welding wire droplet can be precisely controlled to achieve precise control of welding wire deposition. Under the precise and adjustable energy control of the laser, online control of heat input, welding wire deposition efficiency and weld size accuracy can be achieved. Through precise control of energy, welding deformation can be effectively controlled. Through the setting of protective devices, effective welding protection can be achieved. According to the different types of casting defects, the corresponding repair welding groove form is set, and finally the defects of titanium alloy precision castings are repaired. The welding deformation can be controlled to within 0.5mm, which meets the general repair welding requirements of precision castings.

[0045] Specifically, the first preset condition in step S4 includes: The temperature of the high temperature area of ​​laser welding is cooled to below 100°C, and / or, after turning off the laser, the shielding gas is continuously input for more than 30 seconds.

[0046] Through the above arrangement, the weld and the high temperature area near it can be cooled in the atmosphere of protective gas, thereby avoiding oxidation of the weld and the surrounding area, preventing impurities such as nitrogen and oxygen from entering the weld, and maintaining the temperature of the welding area stable, so that the weld can be cooled evenly, reducing cooling deformation and cracking. It should be noted that the high temperature area generally refers to the weld area.

[0047] In summary, the repair method provided in this embodiment has the following advantages over the prior art: 1. This method can realize rapid repair and molding of titanium alloy precision castings with high repair efficiency; 2. By adjusting the output waveform, power, defocusing amount and other parameters of the laser beam, precision welding of titanium alloy castings of different specifications can be achieved, and the process applicability is good; 3. The concentric double ring light spot has a good melting effect on the root of the casting groove, which is conducive to the uniform separation of energy at the bottom, which not only improves the welding wire deposition efficiency, but also improves the root weld quality; 4. It can realize the precision welding repair of titanium alloy castings. There is no introduction of arc or other heat sources in the whole welding process, which is conducive to reducing welding deformation. The welding deformation is less than 0.5mm and the repair quality is high.

[0048] It should be noted that all the terms used in the present invention to indicate directionality and position, such as "upper", "lower", "left", "right", "front", "back", "vertical", "horizontal", "inner", "outer", "top", "lower", "tail end", "head end", "center", etc., are only used to explain the relative positional relationship and connection status between the components in a certain state, and are only for the convenience of describing the present invention, rather than requiring the present invention to be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the descriptions of "first", "second", etc. in the present invention are only used for descriptive purposes, and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features.

[0049] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A concentric wire feeding protection device for laser welding of titanium alloy castings, characterized in that: The invention comprises a protective cover shell (3), a perforated conical plate (4) and a plasma suppression device, wherein a hollow first chamber is enclosed between the protective cover shell (3) and the perforated conical plate (4), the perforated conical plate (4) is arranged on the inner side of the protective cover shell (3), and the perforated conical plate (4) is enclosed to form a second chamber with upper and lower openings, the second chamber being a frustum-shaped chamber that gradually shrinks from top to bottom. During laser welding, a laser beam (5) and a welding wire (6) coaxially pass through the second chamber for welding, and a protective air inlet pipe (7) is arranged on the protective cover shell (3). The protective air inlet pipe (7) is used to transport protective gas into the first chamber. A bottom plate with holes (13) is provided at the bottom of the first chamber. A plurality of first air holes are provided on the bottom plate with holes (13). A plurality of second air holes are provided on the perforated conical plate (4). The second air holes connect the first chamber with the second chamber and are used to introduce the protective gas in the first chamber into the second chamber. The plasma suppression device is provided through the second chamber and is used to blow away negative substances (10) around molten droplets (9) formed by melting of the welding wire (6) during laser welding.

2. The titanium alloy casting laser welding concentric wire feeding protection device according to claim 1, characterized in that: The plasma suppression device comprises a side blowing air inlet pipe (1) and a side blowing pipe (2), wherein the side blowing pipe (2) is arranged through the second chamber, a first end of the side blowing pipe (2) is connected to the side blowing air inlet pipe (1), and a second end is arranged near the periphery of a molten droplet (9) of a welding wire (6) during laser welding, the side blowing air inlet pipe (1) is used to transport side blowing gas into the side blowing pipe (2), and the side blowing pipe (2) is used to use the side blowing gas to blow away negative substances (10) generated during the laser welding process.

3. The concentric wire feeding protection device for laser welding of titanium alloy castings according to claim 2 is characterized in that: More than two side blowing pipes (2) are provided, and the more than two side blowing pipes (2) are evenly distributed around the axial direction of the welding wire (6).

4. The concentric wire feeding protection device for laser welding of titanium alloy castings according to claim 1, characterized in that: A perforated partition plate (8) is also horizontally arranged in the first chamber, the perforated partition plate (8) is used to divide the space in the first chamber, and a plurality of third air holes are arranged on the perforated partition plate (8), the third air holes are used to connect the space divided by the perforated partition plate (8) in which the third air holes are located.

5. The concentric wire feeding protection device for laser welding of titanium alloy castings as claimed in claim 4 is characterized in that: The perforated partition plates (8) are provided in 1 to 3 layers. When two or more layers are provided, the third air holes on adjacent perforated partition plates (8) are arranged in a staggered manner.

6. A precision repair method for titanium alloy castings, using the titanium alloy casting laser welding concentric wire feeding protection device as described in any one of claims 1 to 5, characterized in that: The precision repair method comprises: Step S1: Beveling the casting surface at defective locations, and degreasing and cleaning the area to be welded; Step S2: delivering shielding gas from the shielding gas inlet pipe to the first chamber so that the high-temperature area during the laser welding process is within the protection range of the shielding gas, and delivering side-blowing gas to the plasma suppression device to blow away negative substances generated during the laser welding process; Step S3: setting welding parameters and starting laser welding. During the welding process, shielding gas and side blowing gas are continuously input; Step S4: After reaching the welding end position, turn off the laser beam, turn off the side blowing gas, maintain the shielding gas input until the first preset condition is reached, turn off the shielding gas, and end the welding.

7. The precision repair method according to claim 6, characterized in that: The groove in step S1 is an inverted trapezoidal structure, the groove bottom width a is consistent with the welding spot width, the groove depth C is consistent with the defect depth, transition angles with a radius of R are set on both sides of the groove bottom, and the groove upper opening width b is greater than a3mm-5mm.

8. The precision repair method according to claim 6, characterized in that: In step S3, the laser beam used for welding is a concentric pulsed double annular spot, the laser power of the outer annular spot is smaller than the laser power of the inner annular spot, the outer annular spot is used to preheat the base material near the weld, and the inner annular spot is used for laser welding.

9. The precision repair method according to claim 7, characterized in that: In step S3, the welding parameters include: the laser beam spot is one of circular, rectangular, triangular, elliptical, figure 8, and trapezoidal, the laser power of the outer ring spot is 2000W-4000W, the laser power of the inner ring spot is 6000W-15000W, the defocus is -10mm-10mm, the wire feeding speed is 0.4m / min-3m / min, the welding speed is 0.6m / min-2.0m / min, and the welding wire is placed in the center of the spot shape.

10. The precision repair method according to claim 6, characterized in that: The first preset condition in step S4 includes: the temperature of the high temperature area of ​​laser welding is cooled to below 100° C., and / or, after the laser is turned off, the shielding gas is continuously input for more than 30 seconds.

Citation Information

Patent Citations

  • Protective device for laser welding

    CN102069304A

  • Laser welding method for eliminating back surface splash

    CN107971632A

  • Gas protection device for laser welding

    CN109773333A

  • Protecting device for high power laser welding of thick plate titanium alloy

    CN113305438A

  • Double-ring-shaped laser center wire feeding additive system and control method

    CN116275525A

Cited By

  • Underwater laser coaxial fuse repairing device and method based on energy controllability

    CN119897597A

  • New energy automobile part laser welding platform

    CN122033425A