Reduced ilmenite-based titanium flux-cored wire and preparation method thereof

By controlling the ratio of Mn, Si, FeO in reducing ilmenite and matching specific auxiliary materials, the problem of poor quality of titanium flux-core welding wire is solved, and low-cost and high-performance titanium flux-core welding wire is realized, especially at low temperatures In terms of impact toughness, it achieves an effect that is consistent with rutile.

CN119035868AActive Publication Date: 2024-11-29TIANJIN GOLDEN BRIDGE WELDING MATERIALS GRP CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310613223.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-11-29
Estimated Expiration
2043-05-29

AI Technical Summary

Technical Problem

In the prior art, titanium-type flux-core welding wire prepared from reducing ilmenite raw materials has poor quality, insufficient low-temperature impact toughness, and high cost, making it difficult to effectively replace high-grade natural rutile.

Method used

Using low-cost reduced ilmenite as the main raw material, high-quality titanium-type flux-core welding wire is prepared by controlling the proportion of Mn, Si, FeO and the compatibility of specific slag-making agents, deoxidants, and fluorides, and improving welding process performance and Mechanical properties, especially low-temperature impact toughness.

Benefits of technology

Titanium-type flux-core welding wire prepared with low-priced reducing ilmenite was achieved, and the welding performance reached a level that was consistent with rutile, which significantly reduced manufacturing costs and improved the low-temperature impact toughness of the welding wire.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035868A_ABST
    Figure CN119035868A_ABST
Patent Text Reader

Abstract

The titanium type flux-cored wire is composed of an outer skin and a flux core, and the flux core comprises the following raw materials of the reduced ilmenite, an alloying agent, a slag former, a deoxidizing agent, fluoride and iron powder; the consumption of each material meets the following relation: sigma Mn / sigma Si = 3-5, and sigma Mn + sigma Si / sigma FeO = 5-7; sigma Mn, Sigma Si and Sigma FeO respectively represent the total mass of Mn, Si and FeO in the material. The low-cost reduced ilmenite serves as a main raw material, through reasonable compatibility of other auxiliary materials, control over the proportion of all the materials, particularly the proportion of Mn, Si and FeO and control over the proportion of two components of the slag former, the finally prepared welding wire is excellent in welding performance and high in toughness, and the low-temperature impact toughness of the welding wire is close to that of a welding wire prepared from rutile.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of welding wires, and in particular relates to a titanium-type flux-cored welding wire based on reduced ilmenite and a preparation method thereof. Background Art

[0002] Titanium flux-cored welding wire is a highly efficient welding material with excellent all-position welding process performance and excellent comprehensive mechanical properties. It is widely used in shipbuilding, bridges, engineering machinery, petrochemical, steel structure manufacturing and other industries. At present, the TiO2 slag-making agent of titanium flux-cored welding wire is mainly natural rutile with a purity of more than 90%. The global natural rutile mineral is in short supply, and only a few countries such as Australia and South Africa can produce it. With the annual mining of natural rutile, high-grade natural rutile is becoming increasingly depleted, causing the price of high-grade natural rutile to soar, which seriously affects the manufacturing cost of titanium flux-cored welding wire.

[0003] Reduced ilmenite was previously mostly used for the coating portion of ilmenite-type welding rods. Due to the high impurity content, there is little prior art involving titanium-type flux-cored welding wires that have high welding process requirements.

[0004] Chinese invention patent CN 103358049A discloses "a flux-cored welding wire prepared with high-titanium slag as the main raw material of powder". This patent uses high-titanium slag to replace rutile to reduce the cost of flux core. The purity of TiO2 in high-titanium slag is close to that of natural rutile, and the content of impurities such as Fe, S, and P is slightly higher than that of natural rutile. Therefore, high-titanium slag can achieve better comprehensive performance by replacing natural rutile. The price of high-titanium slag is lower than that of natural rutile, but much higher than that of reduced ilmenite.

[0005] China's invention patent CN 102328156 A discloses "a reduced ilmenite-type flux-cored welding wire". This patent partially replaces rutile with reduced ilmenite to reduce the cost of the flux core, but it still requires a certain amount of rutile and cannot completely replace it with reduced ilmenite. Moreover, it does not specify the TiO2 purity of the reduced ilmenite, the impurity content of FeO, and the slag-making agent, alloying agent, deoxidizer, etc. that are matched with it. As a result, the low-temperature impact toughness at -20°C is less than 80J, barely meeting the national standard, but far lower than the mechanical properties of the rutile slag system.

[0006] Therefore, developing a type of high-quality titanium flux-cored welding wire prepared with low-cost raw materials such as reduced ilmenite has very important scientific research significance and industrial value. Summary of the invention

[0007] In order to solve the defect of poor quality of titanium-type flux-cored welding wire prepared with reduced ilmenite raw material in the prior art, the present invention aims to develop a titanium-type flux-cored welding wire with reduced ilmenite as the main raw material. Reduced ilmenite is obtained by high-temperature sintering of ilmenite. my country has abundant ilmenite resources and low prices. The price of reduced ilmenite is only about 1 / 3 of the price of natural rutile and 1 / 2 of the price of high-titanium slag. The reduced ilmenite of the present invention has significant cost advantages as the main raw material of titanium-type flux-cored welding wire. Moreover, the titanium-type flux-cored welding wire based on reduced ilmenite of the present invention has achieved significantly improved low-temperature impact toughness.

[0008] The present invention solves the above technical problems through the following technical solutions:

[0009] A titanium-type flux-cored welding wire based on reduced ilmenite consists of an outer skin and a flux core, wherein the flux core comprises the following raw materials: reduced ilmenite, an alloying agent, a slag-forming agent, a deoxidizing agent, a fluoride, and iron powder; and the amount of each material satisfies the following relationship: ∑Mn / ∑Si=3-5, ∑Mn+∑Si / ∑FeO=5-7; ∑Mn, ∑Si, ∑FeO respectively represent the total mass of Mn, Si, and FeO in the material.

[0010] Furthermore, the mass content of Mn in the raw material is 10-17wt%, preferably 13-15wt%, such as 13.5wt%, 14.2wt%, 14.8wt%.

[0011] Furthermore, ∑Mn / ∑Si=3.2-4.5, ∑Mn+∑Si / ∑FeO=5.5-6.8. By controlling the feed ratio of raw materials, the total mass of Mn, Si and FeO is controlled.

[0012] Furthermore, the reduced ilmenite contains TiO2≥58wt%, and FeO≤5.5wt%; preferably, the reduced ilmenite contains TiO2≥60wt%, and FeO≤5.0wt%.

[0013] In the standard YB / T 5141-1993 "Reduced ilmenite powder for welding rods", there are two grades FTH7.20 (TiO2≥54%, FeO≤7.0%) and FTH9.20 (TiO2≥52%, FeO≤9.0%). The inventor found that according to the standard YB / T 5141-1993, the content of FeO in the reduced ilmenite powder is relatively high, and the application of it in welding wire is not conducive to the welding process performance and mechanical properties. The inventor selected reduced ilmenite with TiO2≥58wt% and FeO≤5.5wt%, controlled the FeO content, and controlled the appropriate ratio of Mn, Si, and FeO, which can improve the performance of welding wire, especially the low-temperature impact toughness of welding wire.

[0014] The invention adopts low-cost reduced ilmenite as the main raw material, clarifies various chemical composition indicators of the reduced ilmenite, especially adjusts the ratio of total Mn, FeO and Si in the material, and reasonably matches with specific slag-forming agents and fluorides, so that the prepared titanium flux-cored welding wire has high quality, and the welding process performance and mechanical properties after welding reach the level of titanium flux-cored welding wire using rutile as the raw material, and has excellent all-position welding performance, crack resistance and low-temperature impact toughness.

[0015] Furthermore, the core comprises the following raw materials in parts by mass: 40-70 parts of reduced ilmenite, 15-30 parts of alloying agent, 5-10 parts of slag-forming agent, 1-5 parts of deoxidizing agent, 1-5 parts of fluoride, and 1-30 parts of iron powder.

[0016] Furthermore, the core comprises the following raw materials in parts by mass: 46-65 parts of reduced ilmenite, 20-25 parts of alloying agent, 5-10 parts of slag-forming agent, 3-5 parts of deoxidizing agent, 1-3 parts of fluoride, and 1-30 parts of iron powder.

[0017] Furthermore, the alloying agent is at least two of silicon-manganese alloy, ferrosilicon alloy, electrolytic manganese, ferrotitanium, ferroboron, and titanium-ferroboron, and meets the requirements of ∑Mn+∑Si / ∑FeO, and ∑Mn / ∑Si in the above materials.

[0018] Furthermore, the slag-forming agent is a compound of component A and component B, component A is selected from at least one of zircon sand, quartz sand, and feldspar; component B is selected from at least one of potassium titanate and sodium titanate. Furthermore, the slag-forming agent is component A and component B in a mass ratio of 0.5-2:1, preferably 0.9-1.6:1. According to the compounded slag-forming agent, the strength is improved.

[0019] Furthermore, the deoxidizer is at least one of magnesium powder and aluminum-magnesium alloy powder; the fluoride is at least one of sodium fluoride, sodium fluorosilicate, and potassium fluorosilicate.

[0020] The present invention also provides a method for preparing the titanium-type flux-cored welding wire based on reduced ilmenite, comprising the following steps:.

[0021] The outer skin of the core welding wire is made of SPCC-SD cold-rolled low-carbon steel strip, which is cut into a suitable size and rolled into a "U" shape by a rolling mill forming roller; the configured flux core raw materials are baked and mixed and then added into the "U"-shaped groove of the steel strip in proportion; after drawing, layer winding and packaging, titanium-type flux-cored welding wire is obtained.

[0022] The excellent effect of the present invention lies in that low-cost reduced ilmenite is used as the main raw material, and other auxiliary materials are reasonably matched to control the proportion of each material, especially the proportion between Mn, Si and FeO, and the proportion of the two components of the slag-forming agent, so that the welding wire with excellent welding performance, high strength and low-temperature impact toughness close to that of the welding wire made of rutile is finally obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Photo of titanium type flux-cored welding wire based on reduced ilmenite prepared by the present invention. DETAILED DESCRIPTION

[0024] To make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be described in detail below. The following examples are convenient for better understanding of the present invention, but are not intended to limit the present invention. The experimental methods in the following examples are conventional methods unless otherwise specified.

[0025] Example

[0026] Titanium-type flux-cored welding wire was prepared according to the components and amounts in Table 1.

[0027] Reduced ilmenite, TiO2 content 60.2%, FeO content 5%,

[0028] The silicon-manganese alloy is FeMn68Si18, GB / T 4008-2008, in which the Mn content is 68% and the silicon content is 18%;

[0029] The iron silicon alloy is FeSi75-A, GB / T 2272-2009, with a Si content of 75%;

[0030] Electrolytic manganese, DJMnG, YB / T 051-2015;

[0031] Ferrotitanium alloy, FeTi40-A, GB / T 3282-2012;

[0032] Ferroboron alloy, FeB12, GB / T 5682-2015;

[0033] Aluminum-magnesium alloy, FLM1, GB / T 5150-2004;

[0034] Table 1 Titanium flux-cored welding wire composition

[0035]

[0036] The following performance tests were performed on the above embodiments and comparative examples, and the results are shown in Table 2 below.

[0037] The flux-cored welding wire products are tested according to the technical requirements of GB / T 10045-2018 "Non-alloy steel and fine grain steel flux-cored welding wire":

[0038] Tensile strength (Rm): 490~670MPa

[0039] Yield strength (Rel): ≥390MPa

[0040] Elongation after break (A): ≥18%

[0041] -20℃ impact absorption energy (KV2): ≥27J

[0042] Table 2 Flux-cored welding wire deposited metal performance test

[0043] Welding wire samples Rm(MPa) Rel(MPa) A(%) KV2(J, -20℃) Example 1 572 503 24.5 108 Example 2 564 493 26 115 Example 3 552 481 26 143 Example 4 542 472 27 148 Example 5 553 484 26.5 152 Example 6 545 473 25.5 135 Comparative Example 1 548 475 27.5 112 Comparative Example 2 556 482 28 128 Comparative Example 3 493 425 26.5 55 Comparative Example 4 658 586 20.5 48

[0044] From the data in Table 2, it can be found that by matching appropriate raw materials, especially by ensuring the Mn mass content, by adjusting the composite ratio of Mn, Si and FeO to a certain extent, the welding performance of the welding wire can be significantly improved, especially the -20℃ impact absorption energy. The performance has reached that of the welding wire made of expensive rutile as raw material, but the manufacturing cost is significantly reduced.

[0045] In Comparative Example 3, due to the low Mn content, ∑Mn / ∑Si is too low, ∑Mn+∑Si / ∑FeO is too low, and the deoxidation capacity is insufficient, resulting in low tensile strength and a serious decrease in impact toughness.

[0046] In Comparative Example 4, due to the excessively high Mn content, ∑Mn / ∑Si is too high, ∑Mn+∑Si / ∑FeO is too high, and the deoxidation capacity is too high, resulting in excessively high tensile strength and a serious decrease in impact toughness.

Claims

1. A titanium-type flux-cored welding wire based on reduced ilmenite, consisting of an outer sheath and a flux core, characterized in that: The core comprises the following raw materials: reduced ilmenite, alloying agent, slag-making agent, deoxidizing agent, fluoride and iron powder; and the amount of each material satisfies the following relationship: ∑Mn / ∑Si=3-5, ∑Mn+∑Si / ∑FeO=5-7; ∑Mn, ∑Si and ∑FeO respectively represent the total mass of Mn, Si and FeO in the material.

2. The titanium type flux-cored welding wire according to claim 1, characterized in that: The mass content of Mn in the raw material is 10-17wt%, preferably 13-15wt%.

3. The titanium type flux-cored welding wire according to claim 1, characterized in that: ∑Mn / ∑Si=3.2-4.5, ∑Mn+∑Si / ∑FeO=5.5-6.

8.

4. The titanium type flux-cored welding wire according to claim 1, characterized in that: The reduced ilmenite contains TiO2≥58wt%, and FeO≤5.5wt%; preferably, the reduced ilmenite contains TiO2≥60wt%, and FeO≤5.0wt%.

5. The titanium type flux-cored welding wire according to claim 1, characterized in that: The core comprises the following raw materials in parts by mass: 40-70 parts of reduced ilmenite, 15-30 parts of alloying agent, 5-10 parts of slag-forming agent, 1-5 parts of deoxidizing agent, 1-5 parts of fluoride, and 1-30 parts of iron powder.

6. The titanium type flux-cored welding wire according to claim 1, characterized in that: The core comprises the following raw materials in parts by mass: 46-65 parts of reduced ilmenite, 20-25 parts of alloying agent, 5-10 parts of slag-forming agent, 3-5 parts of deoxidizing agent, 1-3 parts of fluoride, and 1-30 parts of iron powder.

7. The titanium type flux-cored welding wire according to claim 1, characterized in that: The alloying agent is at least two of silicon-manganese alloy, ferrosilicon alloy, electrolytic manganese, ferrotitanium, ferroboron and titanium-ferroboron.

8. The titanium type flux-cored welding wire according to claim 1, characterized in that: The slag-forming agent is a compound of component A and component B, wherein component A is selected from at least one of zircon sand, quartz sand, and feldspar; and component B is selected from at least one of potassium titanate and sodium titanate. Furthermore, the slag-forming agent is a compound of component A and component B in a mass ratio of 0.5-2:1, preferably 0.9-1.6:

1.

9. The titanium type flux-cored welding wire according to claim 1, characterized in that: The deoxidizer is at least one of magnesium powder and aluminum-magnesium alloy powder; the fluoride is at least one of sodium fluoride, sodium fluorosilicate and potassium fluorosilicate.

10. The method for preparing the titanium type flux-cored welding wire according to any one of claims 1 to 9, characterized in that The following steps are involved: The outer skin of the core welding wire is made of SPCC-SD cold-rolled low-carbon steel strip, which is cut into a suitable size and rolled into a "U" shape by a rolling mill forming roller; the configured flux core raw materials are baked and mixed and then added into the "U" groove of the steel strip in proportion; after drawing, layer winding and packaging, titanium-type flux-cored welding wire is obtained.

Citation Information

Patent Citations

  • Low alloy steel flux-cored welding wire for carbon dioxide gas protection welding

    CN101104232A

  • Flux-cored wire

    CN101695798A

  • Titanic iron ore type E308 flux-cored wire

    CN109894767A

  • Flux-cored wire for welding low-strength steel and preparation method of flux-cored wire

    CN115846937A

  • Chromium-molybdenum-seel flux welding wire

    CN1358605A