Ni-Cr-P series nickel-based brazing filler metal and preparation method and brazing method thereof

By doping Y elements into Ni-Cr-P-based nickel-based brazing and adopting rapid solidification technology, the problem of phosphide brittle phase in traditional BNi-7 brazing is solved, and the high degree of nickel-based brazing welding joints is achieved Improved mechanical properties and safety.

CN119035871APending Publication Date: 2024-11-29TAIZHOU UNIV (ZHEJIANG)
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411408897.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

During the brazing process, due to the low diffusion coefficient of P element, a complex phosphide brittle phase is formed in the center of the weld, which affects the mechanical properties at the weld and the safety of the components.

Method used

By doping an appropriate amount of Y element into the Ni-Cr-P-based nickel-based brazing material and using rapid solidification technology, amorphous nickel-based brazing material is obtained, which improves the fluidity and composition uniformity of the brazing material and reduces phosphides The generation of brittle phase.

Benefits of technology

It significantly improves the mechanical properties of the brazed joints, and the shear strength can reach 146.08~227.87MPa, enhancing the safety of components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005077445040000091
    Figure BDA0005077445040000091
  • Figure HDA0005077445060000011
    Figure HDA0005077445060000011
  • Figure HDA0005077445060000012
    Figure HDA0005077445060000012
Patent Text Reader

Abstract

The invention provides Ni-Cr-P series nickel-based brazing filler metal as well as a preparation method and a brazing method thereof, and belongs to the technical field of welding materials. The preparation method of the Ni-Cr-P series nickel-based brazing filler metal comprises the steps that alloy metal is smelted and cooled through the rapid solidification technology; the invention further provides specific components of the brazing filler metal. A proper amount of Y is doped in the Ni-Cr-P series nickel-based brazing filler metal, so that the fluidity of the brazing filler metal is effectively improved, weld joint pores are filled in the brazing process, generation of phosphide brittle phases is reduced, and the mechanical property of a welded joint is improved; the amorphous nickel-based brazing filler metal is obtained by combining a rapid solidification technology, the brazing filler metal is uniform in component and can be smoothly diffused to a base metal, generation of a phosphide brittle phase is further reduced, and the mechanical property of a nickel-based brazing filler metal welding joint is improved. The result of the embodiment shows that the shear strength of a welded joint of the nickel-based brazing filler metal provided by the invention can reach 146.08-227.87 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding materials, and in particular to a Ni-Cr-P series nickel-based solder and a preparation method and a brazing method thereof. Background Art

[0002] Nickel-based alloy is a precipitation-strengthened high-temperature alloy with excellent properties such as high strength, corrosion resistance, high-temperature oxidation resistance, fatigue resistance and creep resistance. It is a key material for manufacturing high-temperature components such as turbine disks, turbine blades and combustion chambers in aircraft engines and power machinery. Brazing is the most commonly used connection process in the manufacturing process of nickel-based high-temperature alloys.

[0003] BNi-7 brazing filler metal is a widely used eutectic brazing filler metal for brazing of nickel-based alloys. It is known as the Ni-Cr-P nickel-based brazing filler metal with the lowest melting point together with BNi-6 brazing filler metal. It has good fluidity and wettability, and there is no penetration of the parent metal grain boundary and infiltration embrittlement during the welding process. However, when using traditional BNi-7 brazing filler metal for brazing, due to the low diffusion coefficient of the P element and the fact that the diffusion of the P element is easily hindered by high-melting-point components, a complex phosphide brittle phase is formed in the center of the weld during the brazing process, which will seriously affect the mechanical properties of the weld, thereby affecting the safety and reliability of the components.

[0004] After research, it was found that doping elements in conventional BNi-7 brazing filler metal can reduce the number of brittle compounds in the brazing seam, thereby improving the joint performance. For example, the prior art "Microstructure and mechanical properties of 316L stainless steel joints brazed by BNi-7 alloyed with different Cu content" discloses that adding Cu elements to Ni-Cr-P nickel-based brazing filler metal can make the brazing filler metal's shear strength reach 120MPa, but the mechanical properties of the obtained Ni-Cr-P nickel-based brazing filler metal welded joint still cannot meet the needs of practical applications; the prior art "Investigation of microstructure evolution and strength mechanism of the Cu coated BNi-7 core-shell structure filler metal" also discloses that adding Cu elements to BNi-7 brazing filler metal can improve the mechanical properties of the brazing filler metal, but it requires a complex Cu coating treatment of the BNi-7 brazing filler metal to achieve the improvement of the brazing filler metal's mechanical properties, and the preparation process is complicated. Summary of the invention

[0005] The object of the present invention is to provide a Ni-Cr-P series nickel-based brazing filler metal and a preparation method and a brazing method thereof. The preparation method provided by the present invention is simple, and the prepared nickel-based brazing filler metal can effectively reduce the brittle phase of the weld when used for brazing, and the obtained welding structure has excellent mechanical properties, thereby improving the safety of the brazing filler metal parts.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] A method for preparing a Ni-Cr-P series nickel-based solder comprises the following steps:

[0008] (1) vacuum melting the alloy raw materials to obtain a nickel-based alloy ingot;

[0009] (2) using a rapid solidification technique to first melt and then cool the nickel-based alloy ingot obtained in step (1) to obtain a Ni-Cr-P nickel-based brazing filler metal;

[0010] Calculated by mass percentage, the Ni-Cr-P series nickel-based solder comprises Ni 75.4-75.5%, Cr 13.9-14%, P 10.2-10.3% and Y 0.2-0.5%.

[0011] Preferably, the composition of the Ni-Cr-P series nickel-based solder includes, by mass percentage, 75.4-75.5% Ni, 13.9-14% Cr, 10.2-10.3% P and 0.2-0.4% Y.

[0012] Preferably, the composition of the Ni-Cr-P nickel-based solder is Ni 75.5%, Cr 14%, P 10.3% and Y 0.2% by mass percentage.

[0013] Preferably, the vacuum degree of vacuum melting in step (1) is 0.03-0.05 Pa, the current of vacuum melting is 50-150 A, and the number of vacuum melting is 3-4 times.

[0014] Preferably, the cooling using rapid solidification technology in step (2) includes: spraying the nickel-based alloy melt onto a high-speed rotating copper wheel.

[0015] Preferably, the rotation linear speed of the copper wheel is 12 to 20 m / s.

[0016] Preferably, the distance between the injection port of the nickel-based alloy melt and the copper wheel is 1 to 2 mm, and the injection pressure is 0.1 to 0.2 MPa.

[0017] The present invention also provides a Ni-Cr-P series nickel-based solder obtained by the preparation method described in the above technical solution, wherein the Ni-Cr-P series nickel-based solder is an amorphous structure.

[0018] The invention also provides a brazing method, which adopts the Ni-Cr-P series nickel-based brazing filler metal for brazing.

[0019] Preferably, the vacuum degree of the brazing is 0.001-0.003 Pa, the temperature of the brazing is 940-1020° C., and the time of the brazing is 5-20 min.

[0020] The invention provides a method for preparing a Ni-Cr-P series nickel-based solder, comprising the following steps: (1) performing vacuum smelting on an alloy raw material to obtain a nickel-based alloy melt; (2) using a rapid solidification technology to first melt and then cool the nickel-based alloy ingot obtained in the step (1) to obtain a Ni-Cr-P series nickel-based solder; in terms of mass percentage, the Ni-Cr-P series nickel-based solder comprises 75.4-75.5% Ni, 13.9-14% Cr, 10.2-10.3% P and 0.2-0.5% Y. The present invention effectively improves the fluidity of the brazing material by doping an appropriate amount of Y into the Ni-Cr-P series nickel-based brazing material. During the brazing process, the highly fluid brazing material can fill the weld pores, reduce the generation of phosphide brittle phases, and improve the mechanical properties of the welded joints. The amorphous nickel-based brazing material is obtained by combining the rapid solidification technology. The brazing material has a uniform composition and is not prone to component segregation, so that the brazing material can diffuse smoothly into the parent material, further reducing the generation of phosphide brittle phases and improving the mechanical properties of the nickel-based brazing joints. The results of the embodiment show that the shear strength of the welded joint of the nickel-based brazing material provided by the present invention can reach 146.08 to 227.87 MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The microstructure of the brazed joint of Example 3;

[0022] Figure 2 The microstructure of the brazed joint of Example 4;

[0023] Figure 3 The microstructure of the brazed joint of Comparative Example 6;

[0024] Figure 4 The microstructure of the brazed joint of Comparative Example 7;

[0025] Figure 5 The microstructure of the brazed joint of Comparative Example 8;

[0026] Figure 6 The microstructure of the brazed joint of Comparative Example 9;

[0027] Figure 7 This is the microstructure of the brazed joint of Comparative Example 10. DETAILED DESCRIPTION

[0028] The present invention provides a method for preparing a Ni-Cr-P series nickel-based solder, comprising the following steps:

[0029] (1) vacuum melting the alloy raw materials to obtain a nickel-based alloy ingot;

[0030] (2) using a rapid solidification technique to first melt and then cool the nickel-based alloy ingot obtained in step (1) to obtain a Ni-Cr-P nickel-based brazing filler metal;

[0031] Calculated by mass percentage, the components of the Ni-Cr-P series nickel-based solder include: Ni 75.4-75.5%, Cr 13.9-14%, P 10.2-10.3% and Y 0.2-0.5%.

[0032] In the present invention, the composition of the Ni-Cr-P series nickel-based solder includes Ni75.4-75.5%, preferably 75.5%, by mass percentage.

[0033] In the present invention, the composition of the Ni-Cr-P series nickel-based solder includes Cr13.9-14%, preferably 14%, by mass percentage.

[0034] In the present invention, the composition of the Ni-Cr-P series nickel-based solder includes P10.2-10.3%, preferably 10.3%, by mass percentage.

[0035] In the present invention, Ni, Cr and P are matrix components of the nickel-based solder.

[0036] In the present invention, the composition of the Ni-Cr-P nickel-based solder includes Y0.2-0.5%, preferably 0.2-0.4%, and more preferably 0.2%, by mass percentage. In the present invention, by limiting the amount of Y element, the fluidity of the solder is further improved, the weld is uniform and well filled, thereby reducing the formation of the weld brittle phase and improving the mechanical properties of the welded joint.

[0037] The present invention performs vacuum melting on alloy raw materials to obtain nickel-based alloy ingots.

[0038] In the present invention, the alloy raw materials preferably include metal single substance Ni, metal single substance Cr, metal single substance P and metal single substance Y; the purity of the metal single substance Ni, metal single substance Cr, metal single substance P and metal single substance Y is preferably above 97%.

[0039] In the present invention, the alloy raw material is preferably ultrasonically cleaned and dried before use. The present invention removes impurities on the surface of the raw material by washing the alloy raw material, thereby avoiding the influence of impurities on the properties of the alloy.

[0040] The present invention has no special limitation on the ultrasonic washing and drying operations, and operations well known to those skilled in the art may be used.

[0041] In the present invention, the vacuum degree of the vacuum melting is preferably 0.03-0.05 Pa, more preferably 0.03 Pa; the current of the vacuum melting is 50-150 A, more preferably 100-150 A; the number of vacuum melting is preferably 3-4 times, more preferably 3 times. In the present invention, by limiting the process parameters of vacuum melting and the number of melting times, the raw materials are fully melted, the raw materials are uniformly mixed, the performance of the solder is further improved, and thus the mechanical properties of the solder welded joint are further improved.

[0042] After vacuum smelting is completed, the present invention preferably grinds the alloy ingot obtained by the smelting to obtain a nickel-based alloy ingot. The present invention removes the unreacted alloy raw materials by grinding to avoid affecting the performance of the alloy.

[0043] After obtaining the nickel-based alloy ingot, the present invention preferably uses induction heating to melt the nickel-based alloy ingot to obtain a nickel-based alloy melt. In the present invention, the current of the induction heating is preferably 250-300A.

[0044] After obtaining the nickel-based alloy melt, the invention adopts a rapid solidification technology to cool the obtained nickel-based alloy melt to obtain a Ni-Cr-P series nickel-based brazing filler metal.

[0045] In the present invention, the cooling by using the rapid solidification technology preferably includes: spraying the nickel-based alloy melt onto a high-speed rotating copper wheel.

[0046] In the present invention, the injection pressure is preferably 0.1-0.2 MPa, more preferably 0.1 MPa; the distance between the injection port and the copper wheel is preferably 1-2 mm, more preferably 1 mm; the rotation speed of the copper wheel is preferably 12-20 m / s, more preferably 12-15 m / s. In the present invention, by controlling the process parameters of the rapid solidification technology, the rapid cooling of the alloy melt is better achieved, and the formation of amorphous solder is promoted.

[0047] In the present invention, the spraying process is preferably measured by an infrared pyrometer; the temperature of the sprayed melt is preferably 900-1000° C., more preferably 900-950° C. In the present invention, by controlling the temperature of the sprayed melt, conditions are provided for the rapid solidification technology, which promotes the smooth progress of the rapid solidification process.

[0048] In the present invention, the thickness of the Ni-Cr-P nickel-based solder is preferably 30-50 μm, more preferably 50 μm; the width of the Ni-Cr-P nickel-based solder is preferably 3.5-5 mm, more preferably 5 mm.

[0049] The invention effectively improves the fluidity of the solder by doping a proper amount of Y into the Ni-Cr-P series nickel-based solder. During the brazing process, the solder with high fluidity can fill the weld pores, reduce the generation of phosphide brittle phases, and improve the mechanical properties of the welded joint. In combination with the rapid solidification technology, an amorphous nickel-based solder is obtained, the solder has uniform composition, is not prone to component segregation, and allows the solder to smoothly diffuse into the base material, further reduces the generation of phosphide brittle phases, and improves the mechanical properties of the nickel-based solder welded joint.

[0050] The present invention also provides a Ni-Cr-P series nickel-based solder prepared by the preparation method described in the above technical solution, wherein the Ni-Cr-P series nickel-based solder is preferably an amorphous structure.

[0051] The Ni-Cr-P series nickel-based solder prepared by the preparation method provided by the present invention has excellent fluidity and uniform composition during welding, can effectively fill welding gaps, reduce the generation of phosphide brittle phases, and improve the mechanical properties of welded joints.

[0052] The present invention also provides a brazing method, which uses the Ni-Cr-P series nickel-based brazing filler metal described in the above technical solution to perform brazing to obtain a brazing sample.

[0053] In the present invention, the brazing method preferably comprises the following steps:

[0054] 1) grinding and ultrasonically cleaning the brazing surface of the GH4169 high temperature alloy sample to obtain an alloy block;

[0055] 2) Ni-Cr-P series nickel-based brazing filler metal and alloy blocks are alternately laid and brazed to obtain a brazing sample.

[0056] In the present invention, the brazing surface of the GH4169 high temperature alloy sample is preferably polished and then ultrasonically cleaned to obtain an alloy block.

[0057] In the present invention, the GH4169 high temperature alloy is preferably a GH4169 nickel-based high temperature alloy purchased from Western Superconducting Co., Ltd., and the size is preferably 10mm×10mm×4mm or 4mm×4mm×4mm. In the present invention, the GH4169 high temperature alloy is a basic material for brazing.

[0058] The present invention has no special limitation on the parameters of the grinding and ultrasonic cleaning, and the grinding and ultrasonic cleaning well known to those skilled in the art can be used.

[0059] The present invention preferably cuts the Ni-Cr-P nickel-based solder into a strip solder with a width of 4 mm. In the present invention, the performance of the brazing structure is further improved by controlling the width of the strip solder.

[0060] In the present invention, the strip solder is preferably ultrasonically cleaned before use. In the present invention, impurities on the surface of the raw material are removed by washing the strip solder to avoid the influence of the impurities on the alloy properties.

[0061] The present invention has no special limitation on the operation of the ultrasonic cleaning, and ultrasonic cleaning well known to those skilled in the art may be used.

[0062] After obtaining the alloy block, the present invention preferably brazes the Ni-Cr-P series nickel-based brazing filler metal and the alloy block alternately to obtain a brazing sample.

[0063] In the present invention, the outermost layer during the alternating laying is an alloy block.

[0064] In the present invention, the number of layers of the strip solder is preferably 2 to 3, more preferably 2. In the present invention, by limiting the number of layers, the brazing effect is further ensured and the mechanical properties of the brazed joint are improved.

[0065] In the present invention, the brazing vacuum is preferably 0.001-0.003 Pa, more preferably 0.003 Pa; the brazing temperature is preferably 940-1020°C, more preferably 940-980°C; the brazing time is preferably 5-20 min, more preferably 5-10 min. In the present invention, by limiting the brazing process parameters, the brazing is ensured to proceed smoothly, the brazing effect is promoted, the generation of brittle phase is further reduced, and the mechanical properties of the brazed joint are improved.

[0066] In the present invention, the heating rate of the brazing temperature is preferably 15-20°C / min, more preferably 15°C / min. In the present invention, by controlling the heating rate of brazing, it is ensured that the brazing material can be heated evenly, and the brazing material is prevented from melting on the outside while remaining in a solid state on the inside, thereby affecting the brazing effect and further improving the mechanical properties of the brazed joint.

[0067] In the present invention, the cooling of the brazing preferably includes two stages: the first stage is preferably lowering the brazing temperature to 200-250°C, and the cooling rate is preferably 10-15°C / min; the second stage is preferably cooling from 200-250°C to room temperature with the furnace. In the present invention, by controlling the cooling rate of the brazing, it is ensured that the brazed joint can be uniformly cooled and solidified, and the mechanical properties of the brazed joint are further improved.

[0068] The present invention effectively controls the brazing process by controlling the process parameters of the brazing process of the brazing filler metal, and the obtained brazing joint has excellent mechanical properties.

[0069] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0070] Example 1

[0071] A method for preparing a Ni-Cr-P series nickel-based brazing filler metal comprises the following steps:

[0072] (1) performing vacuum melting on the alloy raw material for 3 times under the conditions of a vacuum degree of 0.03 Pa and a current of 50 A to obtain a nickel-based alloy ingot;

[0073] (2) using a rapid solidification technique to first melt and then cool the nickel-based alloy ingot obtained in step (1) to obtain an amorphous Ni-Cr-P nickel-based brazing filler metal; wherein the rapid solidification technique is to spray the nickel-based alloy melt onto a high-speed rotating copper wheel; the rotation linear speed of the copper wheel is 12 m / s; the spraying pressure is 0.1 MPa; the distance between the spray port and the copper wheel is 1 mm; and the temperature of the sprayed melt is 980° C.;

[0074] Calculated by mass percentage, the composition of the Ni-Cr-P series nickel-based solder is: Ni 75.5%, Cr 14%, P 10.3% and Y 0.2%.

[0075] Example 2

[0076] The difference between Example 2 and Example 1 is that the composition of the Ni-Cr-P series nickel-based solder is: Ni 75.5%, Cr 13.9%, P 10.2% and Y 0.3%, and the rest is the same as Example 1.

[0077] Example 3

[0078] A brazing method, using the Ni-Cr-P series nickel-based brazing filler metal obtained in Example 1 for brazing, comprises the following steps:

[0079] (1) The brazing surface of a GH4169 high-temperature alloy sample with a size of 10 mm × 10 mm × 4 mm was polished and ultrasonically cleaned to obtain an alloy block;

[0080] (2) The Ni-Cr-P series nickel-based solder is cut into strip solder with a width of 4 mm, and the strip solder is laid alternately with the alloy block and brazed for 10 min under the conditions of vacuum degree of 0.003 Pa and temperature of 980°C to obtain a brazing sample; the heating rate of the brazing temperature is 15°C / min; after the brazing is completed, the cooling of the brazing is divided into two stages, the first stage is cooling to 200°C at a cooling rate of 10°C / min, and the second stage is cooling from 200°C to room temperature in the furnace; the number of layers of the strip solder is 2.

[0081] Figure 1 This is the microstructure of the brazed joint of Example 3. Figure 1 It can be seen that when Y is 0.2wt.%, the amorphous solder prepared has an island-like distribution of the brittle phase, which greatly improves the mechanical properties of the joint.

[0082] Example 4

[0083] The only difference between Example 4 and Example 3 is that the Ni-Cr-P nickel-based brazing filler metal obtained in Example 2 is used for brazing, and the rest is the same as Example 3.

[0084] Figure 2 This is the microstructure of the brazed joint of Example 4. Figure 2 It can be seen that when Y is 0.2wt.%, the amount of brittle phase in the prepared amorphous solder is still small, and the mechanical properties of the brazed joint are high.

[0085] Comparative Example 1

[0086] The difference between Comparative Example 1 and Example 1 is that the Ni-Cr-P series nickel-based solder does not contain Y, and the rest is the same as Example 1.

[0087] Comparative Example 2

[0088] The difference between Comparative Example 2 and Example 1 is that the composition of the Ni-Cr-P series nickel-based solder is: Ni 75.1%, Cr 14%, P 10.3% and Y 0.4%, and the rest is the same as Example 1.

[0089] Comparative Example 3

[0090] The difference between Comparative Example 3 and Example 1 is that the composition of the Ni-Cr-P series nickel-based solder is: Ni 74.7%, Cr 14%, P 10.3% and Y 0.5%, and the rest is the same as Example 1.

[0091] Comparative Example 4

[0092] The difference between Comparative Example 4 and Example 1 is that step (2) is omitted, and the rest is the same as Example 1.

[0093] Comparative Example 5

[0094] The difference between Comparative Example 5 and Comparative Example 3 is that the brazing temperature is 940° C., and the other conditions are the same as Comparative Example 3.

[0095] Comparative Examples 6 to 10

[0096] The difference between Comparative Examples 6 to 10 and Example 3 is that the Ni-Cr-P nickel-based brazing filler metals prepared in Comparative Examples 1 to 5 are used for brazing, and the rest is the same as Example 3.

[0097] Figure 3 The microstructure of the brazed joint of Comparative Example 6. Figure 3 It can be seen that the welded joints of nickel-based alloy brazing filler metals without Y doping contain a large amount of brittle phases and have poor mechanical properties.

[0098] Figure 4 The microstructure of the brazed joint of Comparative Example 7. Figure 4 It can be seen that when the Y content in the solder is 0.4%, the amount of brittle phase increases significantly, which further illustrates the influence of the doping amount of Y element on the mechanical properties of the welded joint.

[0099] Figure 5 The microstructure of the brazed joint of Comparative Example 8. Figure 5 It can be seen that when the Y content in the solder is 0.5%, relatively obvious through cracks appear inside the joint, seriously affecting the mechanical properties of the welded joint, indicating that the higher the content of the doped element Y is, the better the mechanical properties of the welded joint will be.

[0100] Figure 6 The microstructure of the brazed joint of Comparative Example 9. Figure 6 It can be seen that the nickel-based alloy that is not cooled by rapid solidification technology has a crystalline structure, and the amount of brittle phase in the welded joint of the alloy solder is significantly increased compared to the welded joint obtained by welding with amorphous solder. This shows that the rapid solidification technology significantly reduces the amount of brittle phase in the welded joint.

[0101] Figure 7 The microstructure of the brazed joint of Comparative Example 10. Figure 7 It can be seen that changing the brazing temperature will affect the amount of brittle phase in the welded joint, resulting in poor mechanical properties of the welded joint.

[0102] The shear strength of the brazed joints of Examples 3 to 4 and Comparative Examples 6 to 10 was tested using a microcomputer-controlled electronic universal testing machine. The results are shown in Table 1.

[0103] Table 1 Shear strength of brazed joints of Examples 3 to 4 and Comparative Examples 6 to 10

[0104]

[0105] As can be seen from Table 1, the present invention effectively improves the fluidity of the solder by controlling the amount of the doping element Y, and combines the rapid solidification technology to obtain an amorphous nickel-based solder, so that the solder composition is uniform, the generation of phosphide brittle phase is reduced, and the mechanical properties of the nickel-based solder welded joint are improved.

[0106] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a Ni-Cr-P series nickel-based brazing filler metal, The following steps are involved: (1) vacuum melting the alloy raw materials to obtain a nickel-based alloy ingot; (2) using a rapid solidification technique to first melt and then cool the nickel-based alloy ingot obtained in step (1) to obtain a Ni-Cr-P nickel-based brazing filler metal; Calculated by mass percentage, the components of the Ni-Cr-P series nickel-based solder include: Ni 75.4-75.5%, Cr 13.9-14%, P 10.2-10.3% and Y 0.2-0.5%.

2. The preparation method according to claim 1, It is characterized in that Calculated by mass percentage, the components of the Ni-Cr-P series nickel-based solder include: Ni 75.4-75.5%, Cr 13.9-14%, P 10.2-10.3% and Y 0.2-0.4%.

3. The preparation method according to claim 2, It is characterized in that Calculated by mass percentage, the composition of the Ni-Cr-P series nickel-based solder is: Ni 75.5%, Cr 14%, P 10.3% and Y 0.2%.

4. The preparation method according to claim 1, It is characterized in that The vacuum degree of vacuum melting in the step (1) is 0.03-0.05 Pa, the current of vacuum melting is 50-150 A, and the number of vacuum melting is 3-4 times.

5. The preparation method according to claim 1, It is characterized in that The cooling by using rapid solidification technology in step (2) includes: spraying the nickel-based alloy melt onto a high-speed rotating copper wheel.

6. The preparation method according to claim 5, It is characterized in that The rotation linear speed of the copper wheel is 12-20 m / s.

7. The preparation method according to claim 5, It is characterized in that The distance between the injection port of the nickel-based alloy melt and the copper wheel is 1-2 mm, and the injection pressure is 0.1-0.2 MPa.

8. The Ni-Cr-P nickel-based brazing filler metal obtained by the preparation method according to any one of claims 1 to 7, It is characterized in that The Ni-Cr-P series nickel-based solder is an amorphous structure.

9. A brazing method, It is characterized in that The Ni-Cr-P nickel-based brazing filler metal described in claim 8 is used for brazing to obtain a brazing sample.

10. The brazing method according to claim 9, It is characterized in that The vacuum degree of the brazing is 0.001-0.003 Pa, the temperature of the brazing is 940-1020° C., and the time of the brazing is 5-20 min.

Citation Information

Cited By

  • Self-lubricating filamentous nickel-based brazing filler metal and preparation method and application thereof

    CN120133797A