Ceramic biscuit with complex intersecting characteristics, ceramic material and processing method of ceramic biscuit
By using ablable filling materials and CNC program processing on CNC machine tools, the problem of edge collapse caused by cutting force in complex shape processing of silicon carbide ceramic blanks is solved, and the preparation of complex intersecting ceramic blanks is achieved without defects , improves processing efficiency and pass rate.
Patent Information
- Application Number
- CN202310613491.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-29
AI Technical Summary
Silicon carbide ceramic blanks are prone to introduce microcracks and residual stresses during CNC machining, especially at complex intersecting bodies, which cause edge collapse due to downward cutting force, making it difficult to process into complex shape structures.
Using CNC digital machine tools, customized tools and absorbable filling materials, hollow structural features are compiled through CNC programs, and filling materials are removed after high-temperature heating, which solves the edge collapse problem and improves processing efficiency and pass rate.
The defect-free preparation of complex intersecting characteristics ceramic blanks is achieved, the processing efficiency is improved, and the passing rate is ensured, and the problem of edge collapse at the intersecting body connection is solved.
Smart Images

Figure CN119036611A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of engineering ceramic material processing and preparation, and in particular relates to a ceramic blank with complex intersecting characteristics, a ceramic material and a processing method thereof. Background Art
[0002] Silicon carbide ceramics have the characteristics of extremely high hardness and high brittleness, and are generally difficult to process into ceramic materials with complex shapes and structures. However, the large-scale promotion and use of silicon carbide ceramic materials as engineering structural materials depends to a large extent on the processing technology of ceramic samples at the green stage.
[0003] Due to its inherent hardness and brittleness, the silicon carbide ceramic blank stage is prone to processing defects such as micro cracks and residual stress during CNC machining (computer digital controlled precision machining), thus causing material damage. Especially for ceramic blanks with complex intersecting body characteristics, the problem of edge collapse is very likely to occur at the junction of the intersecting bodies due to downward cutting force during the machining process. Therefore, the processing must be carried out in a different way from metal processing and traditional ceramic blank processing. Summary of the invention
[0004] In view of the above technical problems, the present invention provides a method for processing a ceramic blank with complex intersecting features, and processes the blank before sintering. The method sets processing parameters through a CNC digital machine tool and uses customized tools, customized tooling and customized ablative filling materials, and uses CNC program compilation to process the hollow structure features of the intersection of the ceramic blank on the CNC machine tool, thereby effectively solving the problem of edge collapse at the intersection of the ceramic blank with complex intersecting body features during the processing of the ceramic blank.
[0005] Specifically, in a first aspect, the present invention provides a method for processing a ceramic blank having complex intersecting features, comprising: Prepare CNC machining programs for CNC machine tools according to ceramic production model parameters and process requirements, input the prepared CNC machining programs into the CNC control system and set CNC machine tool machining process parameters; Fixing the ceramic blank, and processing the first intersecting feature of the ceramic blank by using the CNC machine tool; Fixing the ablatable filling material, and processing the ablatable filling material using the CNC machine tool to match the first intersecting feature; Assembling the ablatable filling material and the first intersecting feature into a secondary processing component, fixing the component on the CNC machine, and processing the second intersecting feature on the secondary processing component using the CNC machine; The secondary processing component after the second intersecting feature processing is completed is heated at high temperature, and the ablative filling material is taken out after cooling to obtain a ceramic blank with complex intersecting features.
[0006] Preferably, the CNC machine tool processing parameters are set as follows: spindle speed S is 1200-8000 r / min, feed rate F is 300-1800 mm / min, and cutting depth AP is 0.2-4 mm.
[0007] Preferably, the cross-sections of the first intersecting features and the second intersecting features are both circular or polygonal structures, and the polygons are preferably square or triangle.
[0008] Preferably, the material of the ablative filling material is polyurethane, and the density of the ablative filling material is 100-200 kg / m 3 .
[0009] Preferably, the ablative filling material is processed with air guide grooves.
[0010] Preferably, the high temperature heating temperature is 100-150° C., and the heating time is 30-60 min.
[0011] In a second aspect, the present invention provides a ceramic blank having complex intersecting features obtained according to the above processing method.
[0012] In a third aspect, the present invention provides a ceramic material obtained by processing the above-mentioned ceramic blank with complex intersecting features.
[0013] Beneficial Effects The processing method provided by the present invention effectively fills the local hollow structure appearing in the processing technology through the ablative filling material, solves the problem of edge collapse at the characteristic connection of the intersecting bodies of the ceramic blank due to the downward cutting force, improves the processing efficiency and ensures the qualified rate, and realizes the defect-free preparation of the ceramic blank with a hollow structure with complex intersecting characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 The process flow chart of the processing method of the ceramic blank with complex intersecting features according to the present invention; Figure 2 It is a schematic diagram of the components of the green billet processing method according to the present invention; Figure 3 This is a schematic diagram of the ceramic blank structure of Example 1; Figure 4 This is a schematic diagram of the ceramic blank structure of Example 2; Figure 5 This is a physical picture of the processed and formed embodiment 2; Figure 6The left picture is a real picture of the part with edge collapse defect, and the right picture is a real picture of the part formed by the processing method of the present invention; Figure 7 The left picture shows the density of 60kg / m 3 The actual picture of the edge collapse defect of the green billet produced by the ablative filling material. The right picture is the one with a density of 130kg / m 3 Actual picture of the blank produced by processing of ablative filling materials. Reference numerals: 1. Ceramic green body, 2. First penetration feature, 3. Second penetration feature, 4. Ablative filling material. DETAILED DESCRIPTION
[0015] The present invention is further described by way of embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, rather than to limit the present invention.
[0016] The following combination Figure 1 , 2 , exemplarily illustrating the processing method of the ceramic blank with complex intersecting features provided by the present invention, the processing method mainly includes the steps of modeling, programming, program input and parameter setting, ablative filling material processing, intersecting feature processing, assembly, ceramic blank forming and the like.
[0017] (1) Modeling: A sample model and a model of ablative filling material are constructed using three-dimensional software, wherein the sample model includes a blank model and a final sample model.
[0018] (2) Programming. The CNC processing program is compiled according to the model process requirements. The present invention utilizes digital CNC molding technology to process ceramic blanks.
[0019] (3) Program input and parameter setting: Input the compiled CNC machining program into the CNC control system and set the CNC machine tool machining process parameters.
[0020] In some embodiments, the CNC machine tool processing parameters can be set as: spindle speed S is 1200-8000 r / min, feed rate F is 300-1800 mm / min, and cutting depth AP is 0.2-4 mm.
[0021] (4) Processing of the first intersecting feature 2. The ceramic blank 1 is clamped and fixed on the working platform of the CNC machine tool, and a program is called to process the first intersecting feature 2.
[0022] The shape and size of the first intersecting feature 2 can be determined according to the structure of the ceramic blank. In some embodiments, the cross section of the first intersecting feature 2 can be a circular or polygonal structure, and the polygon is preferably a square or a triangle.
[0023] (5) Processing of the ablative filling material 4 . The ablative filling material 4 is fixed on the working platform of the CNC machine tool, and a program is called to process the ablative filling material 4 , ensuring that the shape and precision size of the processed ablative filling material 4 are consistent with the filling feature of the first intersecting feature 2 .
[0024] In some embodiments, the material of the ablative filling material 4 may be polyurethane, and the density of the ablative filling material 4 may be 100-200 kg / m 3 , preferably 130kg / m 3 The ablative filling material 4 needs to have a certain density and elasticity to meet the assembly requirements and effectively support and offset the downward cutting force of the tool during processing. If the density is too low, the filling material cannot play a supporting role and cannot offset the downward cutting force of the tool during processing, causing edge collapse; if the density is too high, it will lose its elasticity and become hard, which is easy to damage the sample during assembly.
[0025] In some embodiments, the ablative filling material 4 is processed with air guide grooves, which can promote the rapid discharge of compressed air during the advancement process of assembling the filling material and the ceramic blank to reduce assembly resistance, thereby preventing the filling material from squeezing the blank during assembly.
[0026] The use of ablative filling materials greatly avoids the problem of edge collapse at the joints of intersecting features of ceramic blanks due to downward cutting force, improves processing efficiency and ensures the pass rate, and realizes defect-free preparation of ceramic blanks with complex intersecting features.
[0027] (6) Assembly. The ablative filling material 4 and the first intersecting feature 2 are assembled into a secondary processing component. The assembly method may be a repair assembly method.
[0028] (7) Processing of the second intersecting feature 3. The assembled blank is clamped and fixed on the working platform of the CNC machine tool, and the program is called to process the second intersecting feature 3 to obtain the intersecting feature required for the sample model. The shape and size of the second intersecting feature 3 are determined according to the structure of the ceramic blank. In some embodiments, the cross-section of the second intersecting feature 3 can be a circular or square, triangular or other polygonal structure.
[0029] (8) Ceramic green blank molding: The secondary processing component after the second intersecting feature 3 is processed is heated at high temperature, and after cooling, the ablative filling material 4 is taken out to obtain a ceramic green blank with a complex intersecting body shape.
[0030] In some embodiments, the high temperature heating temperature may be 100 to 150° C., and the heating time may be 30 to 60 minutes.
[0031] The processing method of the ceramic blank with complex intersecting features provided by the present invention effectively fills the local hollow structure appearing in the processing technology through the ablative filling material, solves the problem of edge collapse at the connection of the intersecting body features of the ceramic blank due to the downward cutting force, improves the processing efficiency and ensures the qualified rate, and realizes the defect-free preparation of the ceramic blank with complex intersecting feature hollow structure and ceramic material.
[0032] The following examples are further listed to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are only examples in a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0033] Example 1
[0034] like Figure 3 As shown, the processing method provided by the present invention is used to prepare a 60×50×50 mm 3 Rectangular ceramic samples, first process the rectangular 60×50mm 2 The first intersecting feature on the side (Φ30mm circular hole), then on the cuboid 60×50mm 2 The second intersecting feature (equilateral triangle with an inscribed circle of Φ22mm) is machined on the upper surface. The steps are as follows: (1) Modeling. Use 3D software to build the blank model, final sample model, and ablative filling material model. (2) Programming. Prepare CNC machining programs according to the model process requirements. (3) Program input and parameter setting. Input the compiled CNC processing program into the CNC control system and set the CNC machine tool process parameters. The processing parameters of the first intersecting feature and the second intersecting feature are: spindle speed S is 2000r / min, feed rate F is 500mm / min, and cutting depth AP is 0.5mm; the processing parameters of the ablative filling material are: spindle speed S is 6000r / min, feed rate F is 1000mm / min, and cutting depth AP is 4mm. (4) Processing of the first intersecting feature: The ceramic blank is clamped and fixed on the working platform of the CNC machine tool, and the program is called to process the first intersecting feature (a circular hole of Φ30 mm). (5) Ablative filling material processing. 3The ablative polyurethane material is clamped and fixed on the working platform of the CNC machine tool, and the program is called to process the Φ30mm feature to ensure that its shape and precision size are consistent with the first intersecting feature. The ablative polyurethane material is processed with an air guide groove. (6) Assembly: Assemble the processed ablative polyurethane material Φ30 mm and the first intersecting body Φ30 mm. (7) Processing of the second intersecting feature. The assembled blank is clamped and fixed on the working platform of the CNC machine tool, and the program is called to process the second intersecting feature (equilateral triangle with an inscribed circle of Φ22 mm) to obtain the intersecting feature required for the sample model. (8) Ceramic green blank molding: The green blank sample after the second intersecting feature processing is heated to 120°C, and after cooling, the shrunken polyurethane material is taken out to obtain a ceramic green blank with a complex intersecting body shape.
[0035] Example 2
[0036] like Figure 4 As shown, the processing method provided by the present invention is used to prepare a 500×300×60mm 3 The complex structure of the rectangular ceramic sample is first processed into 500×60mm 2 The first penetration feature on the side of the sample (circular hole penetration feature), and then in the rectangular 500×300mm 2 The upper surface is processed with lightweight features and second penetration features (including rectangles, waist shapes and triangles). The steps are as follows: (1) Modeling. Use 3D software to build the blank model, final sample model, and ablative filling material model. (2) Programming. Prepare CNC machining programs according to the model process requirements. (3) Program input and parameter setting. Input the compiled CNC processing program into the CNC control system and set the CNC machine tool process parameters. The processing parameters of the first intersecting feature and the second intersecting feature are: spindle speed S is 2000r / min, feed rate F is 500mm / min, and cutting depth AP is 0.5mm; the processing parameters of the ablative filling material are: spindle speed S is 6000r / min, feed rate F is 1000mm / min, and cutting depth AP is 4mm. (4) Processing of the first intersecting feature: The blank is clamped and fixed on the working platform of the CNC machine tool, and the program is called to process the first intersecting feature (circular hole penetration feature). (5) Ablative filling material processing. 3The ablative polyurethane material is clamped and fixed on the working platform of the CNC machine tool, and the program is called to process the circular hole feature to ensure that its shape and precision size are consistent with the first intersecting feature. The ablative polyurethane material is processed with an air guide groove. (6) Assembly: Assemble the processed ablative polyurethane material and the first intersecting body (circular hole penetration feature). (7) Processing of the second intersecting feature. The assembled blank is clamped and fixed on the working platform of the CNC machine tool, and the program is called to process 500×300mm 2 Lightweight features and second penetrating features (including rectangles, waist shapes and triangles) are processed on the upper surface to obtain the intersecting features required for the sample model. (8) Ceramic green blank molding: The green blank sample after the second intersecting feature processing is heated to 120°C, and after cooling, the shrunken polyurethane material is taken out to obtain a ceramic green blank with a complex intersecting body shape.
[0037] Figure 5 This is a physical picture of the processed embodiment 2.
[0038] Comparative Example 1
[0039] The processing technology of this comparative example 1 refers to that of Example 2, with the main difference being that the processing parameters of the CNC machine tool are set as follows: the spindle speed S is 500 r / min, the feed rate F is 2000 mm / min, and the cutting depth AP is 4 mm.
[0040] Due to inappropriate setting of the processing parameters of the CNC machine tool, the blank obtained by processing in this comparative example 1 has edge collapse defects. Figure 6 The left picture is a real picture of the part with edge collapse defects, and the right picture is a real picture of the part formed using the processing method of the present invention.
[0041] Comparative Example 2
[0042] The processing technology of this comparative example 2 refers to that of Example 2, with the main difference being that the density of the ablative filling material is 60 kg / m 3 .
[0043] Figure 7 The left picture shows the density of 60kg / m 3 The actual picture of the edge collapse defect of the green billet produced by the ablative filling material. The right picture is the one with a density of 130kg / m 3 As can be seen from the figure, due to the low density of the ablative filling material, it is difficult to obtain effective support when processing the second intersecting feature in this comparative example 2, resulting in the defect of the blank edge collapse.
[0044] Comparative Example 3
[0045] The processing technology of this comparative example 3 refers to that of Example 2, with the main difference that the density of the ablative filling material is greater than 200 kg / m 3 .
[0046] Since the density of the ablative filling material is too high and the material is too hard, the filling material in Comparative Example 3 cannot be assembled with the first intersecting feature or the blank may break or the sample may be damaged during the assembly process.
[0047] Comparative Example 4
[0048] The processing technology of this comparative example 4 refers to that of the example 1, with the main difference being that the ablative filling material is not used to process the air guide groove.
[0049] Since the ablative filling material is not processed with an air guide groove, the comparative example 4 cannot effectively and quickly discharge the air during the assembly process of the filling material and the first intersecting feature, causing excessive internal stress in the blank and edge collapse.
[0050] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.
Claims
1. A method for processing a ceramic blank having complex intersecting features, characterized in that: include: Prepare CNC machining programs for CNC machine tools according to ceramic production model parameters and process requirements, input the prepared CNC machining programs into the CNC control system and set CNC machine tool machining process parameters; Fixing the ceramic blank, and processing the first intersecting feature of the ceramic blank by using the CNC machine tool; Fixing the ablatable filling material, and processing the ablatable filling material using the CNC machine tool to match the first intersecting feature; Assembling the ablatable filling material and the first intersecting feature into a secondary processing component, fixing the component on the CNC machine, and processing the second intersecting feature on the secondary processing component using the CNC machine; The secondary processing component after the second intersecting feature processing is completed is heated at high temperature, and the ablative filling material is taken out after cooling to obtain a ceramic blank with complex intersecting features.
2. The processing method according to claim 1, characterized in that: The processing parameters of the CNC machine tool are set as follows: the spindle speed S is 1200-8000 r / min, the feed rate F is 300-1800 mm / min, and the cutting depth AP is 0.2-4 mm.
3. The processing method according to claim 1 or 2, characterized in that: The cross-sections of the first intersecting feature and the second intersecting feature are both circular or polygonal structures, and the polygon is preferably a square or a triangle.
4. The processing method according to any one of claims 1 to 3, characterized in that: The material of the ablative filling material is polyurethane, and the density of the ablative filling material is 100-200 kg / m 3 .
5. The processing method according to any one of claims 1 to 4, characterized in that: The ablatable filling material is processed with gas guide grooves.
6. The processing method according to any one of claims 1 to 5, characterized in that: The high temperature heating temperature is 100-150° C., and the heating time is 30-60 minutes.
7. A ceramic green body with complex intersecting features obtained by the processing method according to any one of claims 1 to 6.
8. A ceramic material obtained by processing the ceramic green body with complex intersecting features as claimed in claim 7.
Citation Information
Cited By
Machining method for complex features of integrated ceramic part
CN119635838A
A control method of a ceramic CNC machining process and a CNC machining device
CN122924017A