Optical film with high-precision thickness and preparation method thereof

By controlling the air gap and stretching ratio between the T-DIE die head and the cooling roller, high-precision thickness optical films were prepared, solving the problems of insufficient film thickness accuracy and stretchability, and improving film thickness uniformity and stretching performance.

CN119036799APending Publication Date: 2024-11-29ANHUI HEMEI MATERIALS TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411348378.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing technologies struggle to improve film strength and tensile properties while maintaining film thickness accuracy, particularly in the TOUCH and OPEN modes.

Method used

High-precision thickness optical films are prepared by controlling the air gap between the T-DIE die outlet and the landing point of the cooling roller, combined with the stretching ratios in the MD and TD directions. The process includes steps such as melting and cooling of transparent optical polymers, stretching in the MD and TD directions, and using a specific water-soluble primer coating solution to improve the uniformity and precision of the film.

Benefits of technology

It achieves high-precision thickness uniformity and excellent tensile properties of optical films, reduces the impact of airflow on film thickness, and improves film thickness uniformity and precision.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119036799A_ABST
    Figure CN119036799A_ABST
Patent Text Reader

Abstract

The invention relates to an optical film with high-precision thickness and a preparation method thereof, and the method is characterized in that in an OPEN mode, an air gap between an outlet of a T-DIE die head and a landing point of a cooling roller is controlled, so that the influence of airflow on the thickness of a film sheet is reduced, and the film thickness uniformity of the optical film is improved. And the specific thickness condition of the first film and the TD-direction and MD-direction stretching multiplying power are set, so that the film thickness precision of the optical film is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of optical thin films, and in particular to an optical film with high-precision thickness and a preparation method thereof. Background Art

[0002] In the field of film preparation, especially when using PMMA (polymethyl methacrylate) extrusion melt molding process, we face a challenge: how to simultaneously meet the requirements of film width, thickness uniformity and physical properties. At present, there are two main film forming modes in the industry: TOUCH mode and OPEN mode. The structural diagrams of the TOUCH mode and OPEN mode film forming equipment are shown in the figure below. Figure 1 and Figure 2 shown.

[0003] The characteristic of the TOUCH mode is that it can provide better thickness accuracy, but it requires a higher number of revolutions and uses rigid metal rollers for extrusion calendering. However, the uneven pressure distribution in this mode can easily lead to uneven stress distribution in the product, which in turn makes the product prone to cracking. At the same time, the film prepared by the TOUCH mode has many wrinkles on both sides and is easy to crack, and the possibility of NIP roller cracking is also high.

[0004] On the other hand, the film produced by the OPEN mode is strong, easy to stretch, and not easy to break, but its thickness accuracy is relatively poor. This is an obvious shortcoming for some products that have strict requirements on thickness accuracy.

[0005] Therefore, we are faced with an important challenge: how to improve the strength and stretchability of the film while ensuring the thickness accuracy of the film. Summary of the invention

[0006] In order to solve the above technical problems, the present application provides an optical film with high-precision thickness and a method for preparing the same.

[0007] To achieve the above object, the present application provides a method for preparing an optical film with high-precision thickness, comprising the following steps:

[0008] S1. Place a transparent optical polymer into an extruder, melt it, and transport it to a T-DIE die for extrusion under a vacuum negative pressure environment. After cooling by a cooling roller, the polymer is formed to form a first film. The air gap between the T-DIE die outlet and the landing point of the cooling roller is 20 mm to 100 mm. The thickness of the first film satisfies the following conditions: the thickness of the first film is 100 μm to 1000 μm, the film thickness δ within the middle 30% width of the first film is equal to the average film thickness δ of the first film. 平均 The ratio between them is 1.01-1.1, and the film thickness SD value of the first film is less than 0.5;

[0009] S2, stretching the first film sheet described in step S1 in the MD direction to form a second film sheet;

[0010] S3, coating the water-soluble primer coating liquid onto the second film sheet, and after drying, stretching the second film sheet in the TD direction to form a third film sheet, and cutting to obtain an optical film with high-precision thickness.

[0011] As a further improvement of the present application, in step S1, the air gap between the T-DIE die outlet and the landing point of the cooling roller is 30 mm to 40 mm.

[0012] As a further improvement of the present application, in step S1, the thickness of the first membrane is 140 μm to 200 μm.

[0013] As a further improvement of the present application, in step S1, the transparent optical polymer passes through the three heating zones of the extruder in sequence, the first heating zone is 150℃~195℃, the second heating zone is 195℃~250℃, and the third heating zone is 250℃~280℃; the temperature of the T-DIE die outlet is 265℃; the rotation speed of the cooling roller is 10m / min~35m / min, and the temperature of the cooling medium in the cooling roller is 90℃~110℃.

[0014] As a further improvement of the present application, in step S1, the transparent optical polymer is any one of a PMMA composition, a PET composition, and a PC composition.

[0015] As a further improvement of the present application, in step S1, the PMMA composition is a copolymer formed by a UV absorber, a high molecular polymer containing a carbonate group in the molecular chain, an alkyl methacrylate monomer, a styrene monomer, a phenylmaleimide monomer, and an alkyl acrylate monomer, and the glass transition temperature of the PMMA composition is 100°C to 150°C.

[0016] As a further improvement of the present application, in step S2, the stretching ratio in the MD direction is 1.8 to 2.1 times, and the stretching temperature is 130°C to 150°C.

[0017] As a further improvement of the present application, in step S3, the water-soluble primer coating solution includes, by mass percentage, 2% to 15% polyurethane resin, 0.01% to 5% antioxidant, 0.01% to 5% nano-scale silica particles, 0.0005% to 0.005% wetting agent, 0.0005% to 0.005% pH adjuster and the balance is water.

[0018] As a further improvement of the present application, in step S3, the stretching ratio in the TD direction is 1.8 to 2.1 times, and the stretching temperature is 130°C to 150°C.

[0019] To achieve the above objectives, the present application also provides an optical film with high-precision thickness prepared by the above-mentioned preparation method.

[0020] The beneficial effect of the present application is that the present application provides a method for preparing an optical film with high-precision thickness, which reduces the influence of airflow on the thickness of the film by controlling the air gap between the outlet of the T-DIE die and the landing point of the cooling roller, thereby improving the uniformity of the thickness of the optical film. A specific thickness condition of the first film, as well as the stretching ratios in the TD and MD directions are also set, further improving the thickness accuracy of the optical film. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the structure of the film forming equipment in the TOUCH mode;

[0022] Figure 2 It is a schematic diagram of the film forming equipment structure in OPEN mode;

[0023] Figure 3 is a schematic diagram of the positions of the cooling roller and the T-DIE die head of Example 1;

[0024] Figure 4 is a schematic diagram of the cross-sectional width structure of the first diaphragm of Example 1;

[0025] Figure 5 It is a schematic diagram of the positions of the cooling roller and the T-DIE die head of Example 6. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical scheme and advantages of the implementation of the present invention clearer, the specific implementation methods of the present invention are clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] This embodiment provides a method for preparing an optical film with high-precision thickness, comprising the following steps:

[0029] S1. First, an extruder is set up and the temperature is kept constant, and a transparent optical polymer is placed in the extruder, wherein the transparent optical polymer is a PMMA composition, and is extruded and melt-formed, wherein: along the feeding direction of the material, the extruder is provided with three temperature rising zones, the first temperature rising zone is 175°C, the second temperature rising zone is 225°C, and the third temperature rising zone is 265°C; the PMMA composition is a copolymer formed by a UV absorber, a high molecular polymer containing a carbonate group in the molecular chain, an alkyl methacrylate monomer, a styrene monomer, a phenylmaleimide monomer, and an alkyl acrylate monomer, and the glass transition temperature of the PMMA composition is 120°C.

[0030] Secondly, a gear pump, a metal filter and a T-DIE die are installed at the outlet of the extruder. The molten transparent optical polymer is transported to the T-DIE die through the gear pump and the metal filter for extrusion under a vacuum negative pressure environment. The temperature at the outlet of the T-DIE die is 265°C.

[0031] Finally, the cooling roller is arranged below the outlet of the T-DIE die head. The air gap between the outlet of the T-DIE die head and the landing point of the cooling roller is 32.9 mm. The position diagram of the cooling roller and the T-DIE die head is shown in FIG. Figure 3 As shown, the landing point of the cooling roller is the position where the transparent polymer contacts the cooling roller. The cooling roller is used to cool the extruded transparent optical polymer into a mold. The temperature of the cooling roller is set to 100°C, the speed of the cooling roller is 20m / min, and the T-DIE die head uses a 1.5M T-DIE die head. The transparent polymer coming out of the T-DIE die head is cooled by the cooling roller and then molded to form the first film.

[0032] S2. A traction device is also provided behind the cooling roller to pull out the first film after cooling. The speed of the traction device is set at 20 m / min and it operates in conjunction with the cooling roller.

[0033] A film thickness detector is also provided between the cooling roller and the traction device, which is used to measure the film thickness of the first film pulled out. According to the measured film thickness of the first film, the bolts at the outlet of the T-DIE die are adjusted to control the thickness of the first film to meet the following conditions: the thickness of the first film is 143 μm, and the effective width of the first film is a smooth curve, the average thickness of the first film in the middle of 300 mm to 500 mm is 146 μm, and the thickest thickness on both sides is 180 μm, that is, the film thickness δ in the middle of 30% of the width of the first film is equal to the average film thickness δ of the first film. 平均 The ratio between them is 1.02, the film thickness SD value of the first diaphragm is less than 0.5, and the cross-sectional width structure schematic diagram of the first diaphragm is as follows Figure 4 shown.

[0034] An MD stretching device is arranged after the traction device, including a first hot oven and driving wheels with adjustable speed arranged before and after the first hot oven, to provide power in the forward direction to the film, and the MD stretching ratio is confirmed by the speed ratio of the front and rear driving wheels. The MD stretching device is used to stretch the first film sheet described in step S1 in the MD direction. The temperature of the first hot oven is set to 145°C, and the MD stretching ratio is set to 1.8 times, that is, the rotation speed of the driving wheel at the outlet of the first hot oven is 1.8 times the rotation speed of the driving wheel at the inlet of the first hot oven, so as to form a second film sheet.

[0035] S3. After the MD stretching device, a coating device and a drying device are sequentially arranged, and a water-soluble primer coating liquid is coated on the second film by the coating device, and then the coated second film is dried by the drying device. The water-soluble primer coating liquid can increase the sliding property of the final optical film. Wherein: in terms of mass percentage, the water-soluble primer coating liquid includes 2% to 15% polyurethane resin, 0.01% to 5% antioxidant, 0.01% to 5% nano-scale silica particles, 0.0005% to 0.005% wetting agent, 0.0005% to 0.005% pH adjuster and the balance is water.

[0036] After the drying device, a TD stretching device is provided, including a second hot oven and a circulating clamp stretching unit arranged on both sides of the second hot oven. The circulating clamp stretching unit stretches in a 90° direction with the film forward direction to change the molecular arrangement structure of the film material. The TD stretching device is used to stretch the second film in step S2 in the TD direction. The temperature of the second hot oven is set to 140°C, and the TD stretching ratio is set to 2.0 times to form a third film.

[0037] A cutting device is provided behind the TD stretching device, and the cutting is performed to obtain an optical film with high-precision thickness. The width of the optical film is 2530 mm and the thickness is 40 μm ± 3 μm.

[0038] Example 2

[0039] The difference between this embodiment and embodiment 1 is that the first temperature rising zone is 150°C, the second temperature rising zone is 195°C, the third temperature rising zone is 250°C, the glass transition temperature of the PMMA composition is 100°C, the air gap between the T-DIE die outlet and the landing point of the cooling roller is 20 mm, the temperature of the cooling roller is set to 90°C, the speed of the cooling roller is 5 m / min, the thickness of the first film is 100 μm, the film thickness δ within the 30% width range in the middle of the first film is equal to the average film thickness δ of the first film 平均The ratio between them is 1.01, the temperature of the first hot oven is set to 130°C, the stretching ratio in MD is set to 2.1 times, the temperature of the second hot oven is set to 130°C, and the stretching ratio in TD is set to 1.8 times.

[0040] Example 3

[0041] The difference between this embodiment and embodiment 1 is that the first temperature rising zone is 150°C, the second temperature rising zone is 195°C, the third temperature rising zone is 250°C, the glass transition temperature of the PMMA composition is 150°C, the air gap between the T-DIE die outlet and the landing point of the cooling roller is 100 mm, the temperature of the cooling roller is set to 110°C, the speed of the cooling roller is 35 m / min, the thickness of the first film is 500 μm, the film thickness δ within the 30% width range in the middle of the first film is equal to the average film thickness δ of the first film 平均 The ratio between them is 1.1, the temperature of the first hot oven is set to 150°C, the stretching ratio in MD is set to 2.0 times, the temperature of the second hot oven is set to 150°C, and the stretching ratio in TD is set to 2.1 times.

[0042] Example 4

[0043] The difference between this embodiment and embodiment 1 is that the air gap between the T-DIE die outlet and the landing point of the cooling roller is 30 mm, the thickness of the first film is 140 μm, and the film thickness δ within the middle 30% width range of the first film is equal to the average film thickness δ of the first film. 平均 The ratio between them is 1.05, the stretching ratio in MD is set to 1.9 times, and the stretching ratio in TD is set to 1.9 times.

[0044] Example 5

[0045] The difference between this embodiment and embodiment 1 is that the air gap between the T-DIE die outlet and the landing point of the cooling roller is 40 mm, the thickness of the first film is 200 μm, and the film thickness δ within the middle 30% width range of the first film is equal to the average film thickness δ of the first film. 平均 The ratio between them is 1.08, the stretching ratio in MD is set to 2.0 times, and the stretching ratio in TD is set to 1.8 times.

[0046] Example 6

[0047] The difference between this embodiment and embodiment 1 is that the cooling roller is arranged at the side of the T-DIE die outlet, the air gap between the T-DIE die outlet and the landing point of the cooling roller is 75.76 mm, and the position diagram of the cooling roller and the T-DIE die is as shown in FIG. Figure 5As shown. By comparing this embodiment with embodiment 1, it can be seen that the relative positions of the T-DIE die head and the cooling roller of the present application can be moved, and the positional relationship can be displayed in digital form.

[0048] Comparative Example 1

[0049] The difference between this comparative example and Example 1 is that the air gap between the T-DIE die outlet and the landing point of the cooling roller is 10 mm. At high temperature, the GAP is too narrow, the first film is in contact with the T-DIE die lip, and the small molecule resin is accumulated at the lip, which makes it impossible to stably and continuously mass produce.

[0050] Comparative Example 2

[0051] The difference between this comparative example and Example 1 is that the air gap between the T-DIE die outlet and the landing point of the cooling roller is 150 mm. In the falling process with the air gap, the resin melt will shrink symmetrically toward the middle, i.e., the "neckin" phenomenon. If the air gap is too large, the melt will be affected by the surrounding airflow and will swing irregularly. The side of the first diaphragm will be irregularly wavy and cannot be stretched. The possibility of mass production is low.

[0052] Comparative Example 3

[0053] The difference between this comparative example and Example 1 is that the thickness of the first membrane is 50 μm, and the membrane thickness δ within the middle 30% width range of the first membrane is equal to the average membrane thickness δ of the first membrane. 平均 The ratio between them is 1.2.

[0054] Comparative Example 4

[0055] The difference between this comparative example and Example 1 is that the thickness of the first membrane is 800 μm, and the membrane thickness δ within the middle 30% width range of the first membrane is equal to the average membrane thickness δ of the first membrane. 平均 The ratio between them is 1.5.

[0056] Comparative Example 5

[0057] This embodiment is an optical film prepared in TOUCH mode:

[0058] The acrylic resin composition was melted at 260°C using a twin extruder, and an unstretched film with a width of 1500 mm and an average thickness of 145 μm across the entire width of the first film was prepared at 110°C using a T-die film forming machine and a TOUCH cooling roller. The unstretched film was stretched 2.0 times in the MD direction at a temperature of 145°C, and then stretched 2.0 times in the TD direction at the same temperature using a calender stretching machine to prepare a PMMA film.

[0059] The transmittance of the optical films prepared in the above-mentioned embodiments and comparative examples was tested using conventional methods in the industry, and the film thickness of the optical films prepared in the above-mentioned embodiments and comparative examples was tested using an infrared thickness gauge and the uniformity of the film thickness was calculated. The testing principle of the infrared thickness gauge is as follows: Based on the reflection and absorption characteristics of infrared rays, when infrared rays are irradiated to the surface of the object to be tested, part of the light will be reflected back, while the rest will be absorbed. By accurately detecting and analyzing the intensity and wavelength of the reflected infrared rays, the infrared thickness gauge can accurately calculate the thickness of the object to be tested. In this application, for the optical films prepared in Examples 1 to 6 and Comparative Examples 1 to 5, the full width is used as the reference, and 12 points of an optical film are randomly selected for film thickness testing. Each point is tested 3 times, and a total of 36 data are obtained. The maximum film thickness is found from the 36 data. max , film thickness minimum film thickness min , and calculate the average value of these 36 data to get the average film thickness average , the film thickness uniformity calculation formula is as follows: (film thickness max -Film thickness min ) / (2*film thickness average )*100%.

[0060] The results of the transmittance and film thickness uniformity of the optical films prepared in the above-mentioned Examples 1 to 6 and Comparative Examples 1 to 5 are shown in Table 1:

[0061] Table 1

[0062]

[0063] From the data in Table 1, it can be seen that the performance of the film produced by this process can achieve an optical transmittance of > 90%; the film thickness uniformity of the touch mode production process of mass-produced optical films in the industry is in the range of 2% to 3%; the film thickness uniformity of the open mode is 3% to 4%; and the improved film thickness uniformity of the open mode can be accurate to 0.5% to 1.5%; the smaller the film thickness uniformity, the better the film thickness uniformity.

[0064] The uniformity of optical film thickness is an important indicator of film preparation, which affects the spectral characteristics of optical components and determines the actual effective coating area that can meet the requirements. At the same time, it is also an important indicator of the performance of subsequent optical component devices.

[0065] The technical solution provided by the present application adopts the OPEN mode, which maintains the excellent tensile properties and fracture toughness of the film formed by the OPEN mode, and reduces the influence of the airflow on the thickness of the film by controlling the air gap between the outlet of the T-DIE die head and the landing point of the cooling roller, thereby improving the uniformity of the thickness of the optical film. The specific thickness condition of the first film, as well as the stretching ratios in the TD and MD directions, are also set to further improve the film thickness accuracy of the optical film.

[0066] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

Claims

1. A method for preparing an optical film with high-precision thickness, characterized in that: The steps include: S1. Place a transparent optical polymer into an extruder, melt it, and transport it to a T-DIE die for extrusion under a vacuum negative pressure environment. After cooling by a cooling roller, the polymer is formed to form a first film. The air gap between the T-DIE die outlet and the landing point of the cooling roller is 20 mm to 100 mm. The thickness of the first film satisfies the following conditions: the thickness of the first film is 100 μm to 1000 μm, the film thickness δ within the middle 30% width of the first film is equal to the average film thickness δ of the first film. 平均 The ratio between them is 1.01-1.1, and the film thickness SD value of the first film is less than 0.5; S2, stretching the first film sheet described in step S1 in the MD direction to form a second film sheet; S3, coating the water-soluble primer coating liquid onto the second film sheet, and after drying, stretching the second film sheet in the TD direction to form a third film sheet, and cutting to obtain an optical film with high-precision thickness.

2. The preparation method according to claim 1, characterized in that: In step S1, the air gap between the T-DIE die outlet and the landing point of the cooling roller is 30 mm to 40 mm.

3. The preparation method according to claim 1, characterized in that: In step S1, the thickness of the first membrane is 140 μm to 200 μm.

4. The preparation method according to claim 1, characterized in that: In step S1, the transparent optical polymer passes through the three heating zones of the extruder in sequence, the first heating zone is 150°C to 195°C, the second heating zone is 195°C to 250°C, and the third heating zone is 250°C to 280°C; the temperature of the T-DIE die outlet is 265°C; the rotation speed of the cooling roller is 10m / min to 35m / min, and the temperature of the cooling medium in the cooling roller is 90°C to 110°C.

5. The preparation method according to claim 1, characterized in that: In step S1, the transparent optical polymer is any one of a PMMA composition, a PET composition, and a PC composition.

6. The preparation method according to claim 5, characterized in that: In step S1, the PMMA composition is a copolymer formed by a UV absorber, a high molecular polymer containing a carbonate group in the molecular chain, an alkyl methacrylate monomer, a styrene monomer, a phenylmaleimide monomer, and an alkyl acrylate monomer, and the glass transition temperature of the PMMA composition is 100°C to 150°C.

7. The preparation method according to claim 1, characterized in that: In step S2, the stretching ratio in the MD direction is 1.8 to 2.1 times, and the stretching temperature is 130°C to 150°C.

8. The preparation method according to claim 1, characterized in that: In step S3, the water-soluble primer coating solution includes, by weight percentage, 2% to 15% polyurethane resin, 0.01% to 5% antioxidant, 0.01% to 5% nano-scale silica particles, 0.0005% to 0.005% wetting agent, 0.0005% to 0.005% pH adjuster, and the balance is water.

9. The preparation method according to claim 1, characterized in that: In step S3, the stretching ratio in the TD direction is 1.8 to 2.1 times, and the stretching temperature is 130°C to 150°C.

10. An optical film with high-precision thickness prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Resin film as well as preparation method and application thereof

    CN120795523A