Advanced packaging structure and method of micro-electro-mechanical component

By using deep reactive ion etching or wet chemical etching in microelectromechanical component packaging, the problems of low packaging accuracy and insufficient performance caused by traditional metal wire bonding are solved, and higher packaging quality and electric heating efficiency are achieved. Reduced production costs.

CN119038486APending Publication Date: 2024-11-29ASE (KUNSHAN) INC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411051096.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Metal wire bonding technology in traditional microelectromechanical component packaging leads to low packaging accuracy and easy deformation, affecting product quality and production yield, and insufficient electrical and thermal performance, limiting the application range and performance of the components.

Method used

The substrate is etched by deep reactive ion etching or wet chemical etching, and the sealing ring is installed, and the alignment bond is connected. The electrical contacts are exposed through grinding and cutting, forming a PI passivation layer, connecting the copper column bumps and electroplating, and finally passing through Reflow completes the package.

Benefits of technology

It improves packaging accuracy and quality, shortens production cycle, reduces production costs, and improves electric and heating efficiency and component reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038486A_ABST
    Figure CN119038486A_ABST
Patent Text Reader

Abstract

The invention discloses an advanced packaging structure and method of a micro-electro-mechanical component, and belongs to the technical field of micro-electro-mechanical component packaging. The packaging method comprises the following steps: S1, etching; s2, sealing is conducted; s3, performing merging; s4, grinding; s5, cutting is conducted; s6, passivation is carried out; s7, pre-welding treatment is carried out; and S8, reflow soldering. According to the invention, various problems caused by wire shape deformation caused by glue pouring in metal wire bonding in traditional packaging are avoided, and the cost and the yield of product quality are remarkably improved. The packaging method has the advantages of being short in production period, light, thin, short and small in packaging, large in input and output (I / O) number and good in electric heating efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of micro-electromechanical element packaging, and in particular relates to an advanced packaging structure and method of micro-electromechanical elements. Background Art

[0002] In the traditional packaging process of MEMS components, metal wire bonding technology is usually used, followed by package filling, and finally the packaging is completed through a grinding process. However, this process has some obvious defects. The metal wire used in metal wire bonding technology is very thin, which makes it very easy to deform and shift during the package filling process. This deformation not only affects the alignment accuracy of the MEMS components, but also greatly reduces the quality and production yield of the final product. In addition, metal wire bonding technology may also cause deficiencies in the electrical and thermal properties of the packaged components, limiting the application range and performance of the components. Summary of the invention

[0003] In view of the above situation, in order to overcome the defects of the prior art, the present invention proposes a new micro-electromechanical component packaging method. The method can not only improve the accuracy and quality of packaging, but also shorten the production cycle, reduce production costs, and improve the electrothermal efficiency of packaging and the reliability of components.

[0004] In order to achieve the above object, the following technical solution is adopted: The present invention provides an advanced packaging method of micro-electromechanical components, comprising the following steps:

[0005] S1. Etching: etching the substrate by deep reactive ion etching or wet chemical etching to etch out alignment bonds on the substrate;

[0006] S2, sealing; installing a sealing ring on the etched substrate;

[0007] S3, merging; connecting the alignment bonds on the substrate with the corresponding alignment bonds on the silicon wafer;

[0008] S4, grinding: thinning the substrate thickness by grinding;

[0009] S5, cutting: cutting the ground substrate to expose electrical contacts;

[0010] S6, passivation: a PI passivation layer is provided on the surface of the silicon wafer;

[0011] S7, pre-soldering treatment: connect copper pillar bumps to the electrical contacts of the wafer, then deposit Ti / Cu on the copper pillar bumps by physical vapor deposition, then coat photoresist, and then go through exposure, development, electroplating Cu / Ni / SnAg, and wet etching;

[0012] S8, reflow soldering: obtain the packaged product through reflow soldering.

[0013] Furthermore, the reagent used in the wet chemical etching is one of KOH or TMAH.

[0014] Furthermore, the substrate is a glass or silicon substrate.

[0015] Furthermore, the advanced packaging structure of the micro-electromechanical components is obtained by packaging using the packaging method.

[0016] The beneficial effects of the present invention are:

[0017] (1) The present invention avoids the deformation of the wire shape caused by glue filling in the traditional packaging, thereby avoiding various problems derived from the deformation of the wire shape, and significantly improves the cost and product quality yield.

[0018] (2) The packaging method of the present invention has the advantages of short production cycle, light, thin and short packaging, large number of input and output (I / O) and good electrothermal efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a schematic diagram of the process of the advanced packaging structure and method of micro-electromechanical components of the present invention.

[0020] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention.

[0021] Legend: 1. Glass / silicon substrate; 2. Sealing ring; 3. Electrical contact; 4. MEMS component; 5. Alignment key; 6. Silicon wafer; 7. PI passivation layer; 8. Copper pillar bump. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0024] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.

[0025] Example

[0026] Advanced packaging structure and method for micro-electromechanical components

[0027] The packaging method comprises the following steps:

[0028] S1. Etching: Using deep reactive ion etching technology, the substrate material is precisely etched using an ion beam to form the required alignment bond structure;

[0029] Alternatively, wet chemical etching is used to etch the glass or silicon substrate using potassium hydroxide (KOH) or tetramethylammonium hydroxide (TMAH) as an etchant to form the para-bond;

[0030] Deep reactive ion etching technology uses a combination of chemically active ions and physical bombardment to anisotropically etch substrate materials to form high aspect ratio para-bond structures;

[0031] When wet chemical etching, the choice of KOH or TMAH depends on the chemical properties of the substrate material to achieve the best etching effect;

[0032] The etching rate and depth can be controlled by adjusting the etchant concentration, temperature and etching time.

[0033] After etching, rinse the substrate thoroughly with deionized water or other appropriate solvent to remove all residues that may interfere with subsequent steps.

[0034] During the etching process, the etching rate and etching depth must be controlled to ensure the dimensional accuracy and surface quality of the alignment key;

[0035] During the etching process, in addition to selecting the appropriate etchant, the etching environment, such as temperature, pressure, and etching time, must be precisely controlled to ensure uniformity and accuracy of etching;

[0036] After etching is completed, the substrate needs to be thoroughly cleaned to remove residual etchant and etching products to prevent contamination in subsequent steps;

[0037] S2, Sealing: accurately install the sealing ring on the etched substrate. The sealing ring material must have good elasticity and sealing performance to ensure that the packaged components are isolated from the external environment.

[0038] The installation of the sealing ring must ensure that there are no bubbles or impurities on the contact surface with the substrate to achieve the best sealing effect;

[0039] The material selection of the sealing ring needs to consider its compatibility with the substrate, temperature resistance and chemical resistance;

[0040] S3, merging; accurately aligning and connecting the alignment keys etched on the substrate with the alignment keys on the silicon wafer;

[0041] Use high-precision alignment equipment and vision systems to achieve precise alignment of substrates and silicon wafers;

[0042] S4, grinding: through mechanical or chemical grinding methods, the thickness of the substrate is gradually thinned to achieve the required packaging thickness while maintaining the flatness of the substrate and the integrity of the alignment key;

[0043] S5, cutting: Precision cutting of the ground substrate to expose electrical contacts for subsequent electrical connection;

[0044] S6, passivation: a polyimide (PI) passivation layer is formed on the surface of the silicon wafer to protect the silicon wafer from chemical corrosion and physical damage, while improving the insulation performance of the component;

[0045] The thickness and uniformity of the passivation layer have a significant impact on the performance of the device, so the deposition process of the passivation layer needs to be precisely controlled;

[0046] The passivation layer may require subsequent curing to ensure its stability and performance during the packaging process;

[0047] S7, pre-soldering treatment: connecting copper pillar bumps to the electrical contacts of the wafer to serve as a bridge for electrical connection;

[0048] Depositing a titanium / copper (Ti / Cu) layer on the copper pillar bumps by physical vapor deposition technology to enhance the adhesion and conductivity of the copper pillars;

[0049] Apply photoresist and perform exposure and development to form the pattern required for electroplating;

[0050] Electroplating of Cu / Ni / SnAg layers to further improve the reliability of electrical connections and the strength of solder joints;

[0051] Finally, wet etching is performed to remove excess photoresist and metal layers to complete the pre-welding process;

[0052] The connection of the copper pillar bumps must ensure the reliability of their electrical and mechanical connections with the electrical contacts;

[0053] During the physical vapor deposition (PVD) process, the deposition parameters were controlled to obtain a uniform Ti / Cu layer.

[0054] The exposure and development of photoresist need to be precisely controlled to ensure accurate transfer and resolution of the pattern;

[0055] When electroplating Cu / Ni / SnAg layers, it is necessary to control the electroplating parameters to obtain a uniform and dense metal layer;

[0056] S8, reflow soldering: reflow soldering the processed wafer and the package substrate, and melt the solder and fill it between the electrical contacts and the copper pillar bumps by precisely controlling the temperature and time to form a stable electrical connection;

[0057] After the reflow is completed, the solder joints are cooled and solidified to obtain the final packaged product;

[0058] After reflow, the solder joints can be inspected for quality, including solder joint integrity, solder joint strength, and electrical conductivity.

[0059] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

[0060] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. An advanced packaging method for micro-electromechanical components, characterized in that: The steps include: S1. Etching: etching the substrate by deep reactive ion etching or wet chemical etching to etch out alignment bonds on the substrate; S2, sealing; installing a sealing ring on the etched substrate; S3, merging; connecting the alignment bonds on the substrate with the corresponding alignment bonds on the silicon wafer; S4, grinding: thinning the substrate thickness by grinding; S5, cutting: cutting the ground substrate to expose electrical contacts; S6, passivation: a PI passivation layer is provided on the surface of the silicon wafer; S7, pre-soldering treatment: connect copper pillar bumps to the electrical contacts of the wafer, then deposit Ti / Cu on the copper pillar bumps by physical vapor deposition, then coat photoresist, and then go through exposure, development, electroplating Cu / Ni / SnAg, and wet etching; S8, reflow soldering: obtain the packaged product through reflow soldering.

2. The advanced packaging method of micro-electromechanical components according to claim 1, characterized in that: The reagent used in the wet chemical etching is KOH or TMAH.

3. The advanced packaging method of micro-electromechanical components according to claim 2, characterized in that: The substrate is a glass or silicon substrate.

4. The advanced packaging structure of a micro-electromechanical device according to any one of claims 1 to 3, characterized in that: The packaging is obtained by packaging using the packaging method.

Citation Information

Cited By

  • Method for packaging fan-out micro-electro-mechanical component of micro-electro-mechanical component

    CN121536876A