Iron phosphate, lithium iron phosphate positive electrode material and preparation method and application thereof
By using stirring and sintering technology in the preparation process of iron phosphate, loose iron phosphate powder is formed, combined with the optimization of lithium source and carbon source, the problem of inconvenient transmission of lithium iron phosphate is solved, significantly improved electrochemical performance, suitable for High-performance lithium-ion battery.
Patent Information
- Application Number
- CN202411234273.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, the morphology of iron phosphate is not loose and the pore structure is lacking, which leads to inconvenient transmission of lithium iron phosphate and affects the electrochemical performance.
Iron benzoate was added to the mixed solution of stirred hydrogen peroxide, phosphoric acid and pure water, and the heat-insulating reaction was carried out at 65-75°C. After filtration, sintering, forming loose iron phosphate powder, and lithium iron phosphate was prepared by two-stage sintering method to add lithium The ratio of source to carbon source, ball milling and sintering to improve material performance.
The prepared iron phosphate has a porous structure, which improves the transmission channel of lithium ions and improves the electrochemical performance of lithium iron phosphate, making it suitable for high-performance lithium ion batteries.
Smart Images

Figure CN119038511A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to an iron phosphate, lithium iron phosphate positive electrode material and a preparation method and application thereof. Background Art
[0002] Lithium iron phosphate is one of the most common cathode materials for lithium-ion batteries. It has a stable olivine structure, can reversibly embed and deintercalate lithium ions, and has the advantages of high energy density, stable performance, high safety, and environmental friendliness. It is a highly potential cathode material for lithium-ion batteries. In the preparation process of lithium iron phosphate, the existing technology usually uses iron phosphate to provide iron and phosphorus sources. Therefore, the morphology of iron phosphate has an important influence on the subsequent electrochemical properties of lithium iron phosphate.
[0003] The preparation of iron phosphate usually involves mixing trivalent iron salt with phosphoric acid or soluble phosphate solution, controlling the pH value with ammonia or alkali solution, and crystallizing under heating conditions; or a mixed solution of divalent iron salt and phosphoric acid or soluble phosphate is used, and the reaction conditions are controlled by an oxidant and alkali solution to obtain iron phosphate crystals. However, the iron phosphate prepared by these methods has a poor morphology and does not have a loose pore structure, so the prepared lithium iron phosphate is not conducive to the transmission of lithium ions.
[0004] Based on this, a method for preparing iron phosphate with loose morphology and rich pore structure is provided, and a lithium iron phosphate positive electrode material is prepared based on this. Summary of the invention
[0005] The present invention aims to solve the technical problem that the iron phosphate prepared by the existing method has a poor morphology and does not have a loose pore structure, so that the prepared lithium iron phosphate is not conducive to lithium ion transmission. The purpose is to provide an iron phosphate, lithium iron phosphate positive electrode material and its preparation method and application. The prepared iron phosphate has a loose morphology and more pores, which is suitable for further preparing battery-grade lithium iron phosphate with excellent electrochemical properties. The prepared lithium iron phosphate also has more pores, which provides more channels for the transmission of lithium ions and improves the electrical properties of the lithium iron phosphate.
[0006] The present invention is achieved through the following technical solutions:
[0007] The first object of the present invention is to provide a method for preparing ferric phosphate, comprising the following steps:
[0008] Add ferric benzoate to a mixture of hydrogen peroxide, phosphoric acid and pure water under stirring, and keep the mixture at 65-75° C. for 12-24 hours; wherein the volume ratio of hydrogen peroxide, phosphoric acid and pure water is 1:(2-2.6):10, and 4-6 g of ferric benzoate is added to every 1 mL of hydrogen peroxide;
[0009] The filter cake is filtered out, which is crude ferric phosphate dihydrate, washed with pure water, dried at 80-90°C, sintered, cooled and crushed to obtain finished ferric phosphate powder.
[0010] Furthermore, 5 g of iron benzoate was added to every 1 mL of hydrogen peroxide.
[0011] Furthermore, the sintering method comprises:
[0012] First, nitrogen is introduced and air is exhausted;
[0013] Next, the first stage of sintering is carried out: the temperature is raised to 150-250°C, nitrogen is always introduced during the sintering period, and the sintering is carried out for 3-5 hours;
[0014] Then, the second stage of sintering is carried out: the temperature is raised to 500°C, and sintered at this temperature for 3-6 hours; then kept at 500°C for 12 hours;
[0015] Finally, the mixture was cooled to room temperature under a nitrogen atmosphere, and the cooled product was ground and pulverized to obtain finished iron phosphate powder.
[0016] The second object of the present invention is to provide a method for preparing a lithium iron phosphate positive electrode material, comprising the following steps:
[0017] Weigh a lithium source, an iron source, and a phosphorus source according to a molar ratio of n(Li):n(Fe):n(P)=(1.01-1.05):1:1, and add a carbon source; the iron source and the phosphorus source are prepared using the iron phosphate powder obtained by the above method;
[0018] The prepared materials are ball-milled with deionized water and dried to obtain a powdery precursor;
[0019] The powdered precursor is sintered to obtain a finished lithium iron phosphate positive electrode material.
[0020] Furthermore, the lithium source is at least one of lithium carbonate and lithium hydroxide monohydrate, and the carbon source is at least one of glucose, sucrose, citric acid, polyethylene glycol, carbon nanotubes, graphene, and carbon black.
[0021] Furthermore, the total mass of the carbon source is 3-20% of the mass of the finished lithium iron phosphate positive electrode material.
[0022] Furthermore, the ball milling time is 2h-10h.
[0023] Furthermore, the sintering is a two-stage sintering, and the sintering method includes:
[0024] First, nitrogen is introduced and air is exhausted;
[0025] Next, the first stage of sintering is carried out: the temperature is raised to 300-500°C, nitrogen is introduced at this temperature, and sintering is carried out for 4-6 hours;
[0026] Then, the second stage of sintering is carried out: the temperature is raised to 600-850°C and sintered at this temperature for 6-10 hours;
[0027] Finally, the mixture was cooled to room temperature under a nitrogen atmosphere, and the cooled product was ground and pulverized to obtain a finished lithium iron phosphate positive electrode material.
[0028] The third object of the present invention is to provide a lithium iron phosphate positive electrode material prepared by the above method.
[0029] The third object of the present invention is to provide an application of a lithium iron phosphate positive electrode material, specifically for use in lithium batteries. Based on this, a lithium-ion battery is provided, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet comprises the lithium iron phosphate positive electrode material.
[0030] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0031] The iron phosphate prepared by the present invention has a loose morphology and more pores, and is suitable for further preparing battery-grade lithium iron phosphate with excellent electrochemical performance. The prepared lithium iron phosphate also has more pores, which provides more channels for the transmission of lithium ions and improves the electrical performance of the lithium iron phosphate. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings:
[0033] Figure 1 This is a SEM morphology image of the iron phosphate material prepared in Example 1;
[0034] Figure 2 This is a SEM morphology image of the iron phosphate material prepared in Comparative Example 1;
[0035] Figure 3 This is the SEM morphology of the iron phosphate material prepared in Comparative Example 2. DETAILED DESCRIPTION
[0036] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the technical solutions in the embodiments of the present invention are clearly and completely described below in combination with the embodiments and drawings. Obviously, the schematic implementation modes of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.
[0037] The following is a detailed description of an iron phosphate, lithium iron phosphate positive electrode material, a preparation method and an application thereof of the present invention with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions and repeated descriptions of well-known matters are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art.
[0038] The "range" disclosed in this application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range.
[0039] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0040] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0041] Unless otherwise specified, the terms "include" and "comprising" mentioned in this application may be open-ended or closed-ended. For example, the terms "include" and "comprising" may mean that other substances not listed may also be included or only the listed substances may be included.
[0042] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0043] In order to solve the technical problem that the iron phosphate prepared by the existing method has a poor morphology and does not have a loose pore structure, so that the prepared lithium iron phosphate is not conducive to lithium ion transmission, the technical solution of the present invention is to provide a method for preparing iron phosphate, comprising the following steps:
[0044] Add ferric benzoate to a mixture of hydrogen peroxide, phosphoric acid and pure water under stirring, and keep the mixture at 65-75° C. for 12-24 hours; wherein the volume ratio of hydrogen peroxide, phosphoric acid and pure water is 1:(2-2.6):10, and 4-6 g of ferric benzoate is added to every 1 mL of hydrogen peroxide;
[0045] The filter cake is filtered out, which is crude ferric phosphate dihydrate, washed with pure water, dried at 80-90°C, sintered, cooled and crushed to obtain finished ferric phosphate powder.
[0046] The two oxygen atoms in the hydrogen peroxide molecule carry a negative charge, and there is a repulsive effect between them. This repulsive effect causes the bond angle of the hydrogen peroxide molecule to become 94.5°. This distorted spatial structure makes the hydrogen peroxide molecule highly active. Ferric benzoate is constructed from an iron atom and three benzene rings. The high reactivity of hydrogen peroxide causes hydrogen peroxide to adhere to the surface of iron phosphate when reacting to form iron phosphate. The lone electron of hydrogen peroxide affects the dp-π bonding of the phosphate molecule, making the generated iron phosphate morphology relatively loose. The iron phosphate finally prepared has a loose morphology and more pores, which is suitable for further preparation of battery-grade lithium iron phosphate with excellent electrochemical properties. The prepared lithium iron phosphate also has more pores, providing more channels for the transmission of lithium ions and improving the electrical properties of lithium iron phosphate.
[0047] As a preferred embodiment, 5 g of iron benzoate is added to every 1 mL of hydrogen peroxide;
[0048] As a preferred embodiment, the pure water washing is performed at least twice, preferably three times.
[0049] As a preferred embodiment, the sintering method includes:
[0050] First, nitrogen is introduced and air is exhausted;
[0051] Next, the first stage of sintering is carried out: the temperature is raised to 150-250°C, nitrogen is introduced at this temperature, and sintering is carried out for 3-5 hours;
[0052] Then, the second stage of sintering is carried out: the temperature is raised to 500°C, and sintered at this temperature for 3-6 hours; then kept at 500°C for 12 hours;
[0053] Finally, the mixture was cooled to room temperature under a nitrogen atmosphere, and the cooled product was ground and pulverized to obtain finished iron phosphate powder.
[0054] Based on the iron phosphate powder prepared by the above method, preparing a lithium iron phosphate positive electrode material comprises the following steps:
[0055] Weigh a lithium source, an iron source, and a phosphorus source according to a molar ratio of n(Li):n(Fe):n(P)=(1.01-1.05):1:1, and add a carbon source; the iron source and the phosphorus source are prepared using the iron phosphate powder obtained by the above method;
[0056] The prepared materials are ball-milled with deionized water and dried to obtain a powdery precursor;
[0057] The powdered precursor is sintered to obtain a finished lithium iron phosphate positive electrode material.
[0058] As a preferred embodiment, the lithium source is at least one of lithium carbonate and lithium hydroxide monohydrate, and the carbon source is at least one of glucose, sucrose, citric acid, polyethylene glycol, carbon nanotubes, graphene, and carbon black.
[0059] As a preferred embodiment, the total mass of the carbon source is 3-20% of the mass of the finished lithium iron phosphate positive electrode material, for example, it can be 3%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, etc.
[0060] As a preferred embodiment, the ball milling time is 2h-10h, for example, it can be 2, 3, 4, 5, 6, 7, 8, 10, etc.
[0061] As a preferred embodiment, the sintering is a two-stage sintering, and the sintering method includes:
[0062] First, nitrogen is introduced and air is exhausted;
[0063] Next, the first stage of sintering is carried out: the temperature is raised to 300-500°C, nitrogen is always introduced during the sintering period, and the sintering is carried out for 4-6 hours;
[0064] Then, the second stage of sintering is carried out: the temperature is raised to 600-850°C and sintered at this temperature for 6-10 hours;
[0065] Finally, the mixture was cooled to room temperature under a nitrogen atmosphere, and the cooled product was ground and pulverized to obtain a finished lithium iron phosphate positive electrode material.
[0066] Based on the above method, the present invention also obtains a lithium iron phosphate positive electrode material. The lithium iron phosphate positive electrode material is used in lithium batteries, specifically in lithium ion batteries, the lithium ion batteries include positive electrode sheets, negative electrode sheets, separators and electrolytes, and the positive electrode sheets include the lithium iron phosphate positive electrode material prepared by the present invention.
[0067] The technical solution of the present invention is further described in detail below in conjunction with embodiments.
[0068] It should be noted that the experimental methods used in the examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained by those skilled in the art through commercial channels.
[0069] Example 1
[0070] A method for preparing a lithium iron phosphate positive electrode material:
[0071] (1) Preparation of iron phosphate materials
[0072] Preparation of ferric phosphate dihydrate: prepare a mixed solution of 25 ml 3% hydrogen peroxide, 50 ml 20% phosphoric acid, and 250 ml pure water, add 125 g ferric benzoate to the mixed solution, and keep it at 70°C for 12 hours. Filter, wash the generated solid three times with 250 ml pure water, and dry at 85°C to obtain ferric phosphate dihydrate;
[0073] Sintering: First, nitrogen is introduced and the air is exhausted; the prepared ferric phosphate dihydrate is calcined at 200°C for 3 hours, then the temperature is raised to 500°C for calcination for 4 hours, and then kept at 500°C for 12 hours. Finally, it is cooled to room temperature under a nitrogen atmosphere, and the cooled product is ground to obtain the ferric phosphate material.
[0074] (2) Preparation of lithium iron phosphate positive electrode material
[0075] 200 g of iron phosphate prepared in step (1), 51.46 g of lithium carbonate, 6 g of PEG1500 and 12 g of glucose were mixed in a ball mill for 2 hours. The mixture was spray dried and then sintered. First, nitrogen was introduced and air was exhausted. The mixture was calcined at 400° C. for 4 hours in a nitrogen atmosphere and then heated to 780° C. for 6 hours to obtain a lithium iron phosphate positive electrode material.
[0076] Example 2
[0077] A method for preparing a lithium iron phosphate positive electrode material:
[0078] (1) Preparation of iron phosphate materials
[0079] Preparation of ferric phosphate dihydrate: prepare a mixed solution of 25 ml 3% hydrogen peroxide, 65 ml 20% phosphoric acid, and 250 ml pure water, add 125 g ferric benzoate to the mixed solution, and keep it at 70°C for 20 hours. Filter, wash the generated solid three times with 250 ml pure water, and dry at 90°C to obtain ferric phosphate dihydrate;
[0080] Sintering: First, nitrogen is introduced and the air is exhausted; the prepared ferric phosphate dihydrate is calcined at 250°C for 5 hours, then the temperature is raised to 500°C and calcined for 5 hours, then kept at 500°C for 12 hours, and finally, cooled to room temperature under a nitrogen atmosphere, and the cooled product is ground to obtain the ferric phosphate material.
[0081] (2) Preparation of lithium iron phosphate positive electrode material
[0082] 200 g of iron phosphate prepared in step (1), 51.46 g of lithium carbonate, 6 g of PEG1500 and 12 g of glucose were mixed in a ball mill for 5 hours. The mixture was spray dried and then sintered. First, nitrogen was introduced and air was exhausted. The mixture was calcined at 500° C. for 5 hours in a nitrogen atmosphere and then heated to 820° C. for 8 hours to obtain a lithium iron phosphate positive electrode material.
[0083] Example 3
[0084] A method for preparing a lithium iron phosphate positive electrode material:
[0085] (1) Preparation of iron phosphate materials
[0086] Preparation of ferric phosphate dihydrate: prepare a mixed solution of 25 ml 3% hydrogen peroxide, 70 ml 20% phosphoric acid, and 250 ml pure water, add 125 g ferric benzoate to the mixed solution, and keep it at 70°C for 12 hours. Filter, wash the generated solid three times with 250 ml pure water, and dry at 85°C to obtain ferric phosphate dihydrate;
[0087] Sintering: First, nitrogen is introduced and the air is exhausted; the prepared ferric phosphate dihydrate is calcined at 200°C for 3 hours, then the temperature is raised to 500°C for calcination for 4 hours, and then kept at 500°C for 12 hours. Finally, it is cooled to room temperature under a nitrogen atmosphere, and the cooled product is ground to obtain the ferric phosphate material.
[0088] (2) Preparation of lithium iron phosphate positive electrode material
[0089] 200 g of iron phosphate prepared in step (1), 51.46 g of lithium carbonate, 6 g of PEG1500 and 12 g of glucose were mixed in a ball mill for 2 hours. The mixture was spray dried and then sintered. First, nitrogen was introduced and air was exhausted. The mixture was calcined at 400° C. for 4 hours in a nitrogen atmosphere and then heated to 780° C. for 6 hours to obtain a lithium iron phosphate positive electrode material.
[0090] Example 4
[0091] A method for preparing a lithium iron phosphate positive electrode material:
[0092] (1) Preparation of iron phosphate materials
[0093] Preparation of ferric phosphate dihydrate: prepare a mixed solution of 25 ml 3% hydrogen peroxide, 65 ml 20% phosphoric acid, and 250 ml pure water, add 125 g ferric benzoate to the mixed solution, and keep it at 70°C for 20 hours. Filter, wash the generated solid three times with 250 ml pure water, and dry at 90°C to obtain ferric phosphate dihydrate;
[0094] Sintering: First, nitrogen is introduced and the air is exhausted; the prepared ferric phosphate dihydrate is calcined at 250°C for 5 hours, then the temperature is raised to 500°C and calcined for 5 hours, then kept at 500°C for 12 hours, and finally, cooled to room temperature under a nitrogen atmosphere, and the cooled product is ground to obtain the ferric phosphate material.
[0095] (2) Preparation of lithium iron phosphate positive electrode material
[0096] 200 g of iron phosphate prepared in step (1), 51.94 g of lithium carbonate, 6 g of PEG1500 and 12 g of glucose were mixed in a ball mill for 5 hours. The mixture was spray dried and then sintered. First, nitrogen was introduced and air was exhausted. The mixture was calcined at 500° C. for 5 hours in a nitrogen atmosphere and then heated to 820° C. for 8 hours to obtain a lithium iron phosphate positive electrode material.
[0097] Comparative Example 1
[0098] The difference between this comparative example 1 and example 1 is that the preparation method of the iron phosphate material is different, specifically:
[0099] 556g of ferrous sulfate heptahydrate and 268g of diammonium hydrogen phosphate were mixed and ground for 1 hour, and the ground solid was added to 1000mL of 3% hydrogen peroxide, stirred for 1 hour, filtered, washed with pure water, and dried at 80°C overnight to obtain an iron phosphate material. The iron phosphate material was used to prepare a lithium iron phosphate positive electrode material using the method of Example 1.
[0100] Comparative Example 2
[0101] The difference between this comparative example 2 and example 1 is that the preparation method of the iron phosphate material is different, specifically:
[0102] 400g of ferric nitrate was dissolved in 1000mL of pure water to prepare an aqueous solution of ferric nitrate, and the aqueous solution of ferric nitrate was added to 500mL of 20% phosphoric acid solution, and finally ammonium bicarbonate was added to adjust the pH to 7, at which time the ferric phosphate was precipitated in the form of a solid, filtered, washed with pure water, and dried at 80°C overnight to obtain an ferric phosphate material. The ferric phosphate material was used to prepare a lithium iron phosphate positive electrode material using the method of Example 1.
[0103] The lithium iron phosphate positive electrode materials prepared in Examples 1-4 and Comparative Examples 1-2 were prepared into batteries, and then performance tests were performed. The performance test results are shown in Table 1. The preparation process of the battery is as follows:
[0104] In this experiment, the positive electrode material needs to be configured into a button battery for testing. The specific operations required are as follows: the prepared material is used as the positive electrode, the lithium sheet is used as the negative electrode for battery assembly, 1 mol / L LiPF6 / EC (ethylene carbonate) / DMC (diethyl carbonate) (EC and DMC volume ratio 1:1) is used as the electrolyte, and the diaphragm is a polypropylene microporous membrane. The battery performance is tested using a two-electrode battery test module. The charge and discharge performance test of the positive electrode material is carried out on the battery test system. A constant current charge and discharge system is adopted, the charge and discharge voltage range is 2.0-4.2v, and a 1-minute standstill is set before the constant current process. Among them, the battery assembly is carried out in a glove box with a high-purity argon atmosphere.
[0105] Table 1 Performance test data of batteries prepared from lithium iron phosphate positive electrode materials prepared in Examples 1-4 and Comparative Examples 1-2
[0106]
[0107]
[0108] From the data in Table 1, it can be seen that in Examples 1 and 2, in the 0.1C first charge, the gram capacity of the lithium iron phosphate battery reaches more than 163 mAh / g, and in the 0.1C first discharge, the gram capacity of the lithium iron phosphate battery reaches more than 162 mAh / g, and the data in all aspects are good; while Example 3 increases the addition ratio of phosphoric acid, and Example 4 increases the addition ratio of lithium source, and the electrical performance is reduced to a certain extent compared with Examples 1 and 2.
[0109] Compared with Example 1, Comparative Example 1 replaces iron benzoate with ferrous sulfate heptahydrate, and the iron source used is different. Compared with Example 1, Comparative Example 2 replaces iron benzoate with ferric nitrate. From the data, the electrical properties of Comparative Examples 1 and 2 are significantly reduced, indicating that the present invention uses iron benzoate as the iron source, which is better than other iron sources.
[0110] In addition, the SEM morphologies of the iron phosphate materials prepared in Example 1 and Comparative Example 1 and Comparative Example 2 are as follows: Figure 1 , 2 , 3. By comparison, we can see that Figure 1 The iron phosphate material prepared in Example 1 is obviously looser in morphology, has more pores, and has a smaller particle size, so that the prepared lithium iron phosphate also has a porous structure, providing more channels for the transmission of lithium ions, which is beneficial to improving the electrical properties of lithium iron phosphate.
[0111] Finally, it should be noted that the above specific embodiments are only used to explain in detail the purpose, technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific implementation method of the present invention and is not used to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above specific embodiments, ordinary technicians in this field should understand that it is still possible to modify the technical solutions recorded in the above embodiments, or to replace or improve some or all of the technical features therein. These modifications, equivalent replacements and improvements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and description of the present invention.
Claims
1. A method for preparing iron phosphate, It is characterized in that The following steps are involved: Add ferric benzoate to a mixture of hydrogen peroxide, phosphoric acid and pure water under stirring, and keep the mixture at 65-75° C. for 12-24 hours; wherein the volume ratio of hydrogen peroxide, phosphoric acid and pure water is 1:(2-2.6):10, and 4-6 g of ferric benzoate is added to every 1 mL of hydrogen peroxide; The filter cake is filtered out, which is crude ferric phosphate dihydrate, washed with pure water, dried at 80-90°C, sintered, cooled and crushed to obtain finished ferric phosphate powder.
2. A method for preparing iron phosphate according to claim 1, It is characterized in that Add 5g of iron benzoate to every 1mL of hydrogen peroxide.
3. A method for preparing iron phosphate according to claim 1, It is characterized in that The sintering method comprises: First, nitrogen is introduced and air is exhausted; Next, the first stage of sintering is carried out: the temperature is raised to 150-250°C, nitrogen is always introduced during the sintering period, and the sintering is carried out for 3-5 hours; Then, the second stage of sintering is carried out: the temperature is raised to 500°C, and sintered at this temperature for 3-6 hours; then kept at 500°C for 12 hours; Finally, the mixture was cooled to room temperature under a nitrogen atmosphere, and the cooled product was ground and pulverized to obtain finished iron phosphate powder.
4. A method for preparing a lithium iron phosphate positive electrode material, It is characterized in that The following steps are involved: A lithium source, an iron source, and a phosphorus source are weighed and mixed according to a molar ratio of n(Li) ∶ n(Fe) ∶ n(P) = (1.01-1.05) ∶ 1 ∶ 1, and a carbon source is added; the iron source and the phosphorus source are iron phosphate powders prepared by the method according to any one of claims 1 to 3; The prepared materials are ball-milled with deionized water and dried to obtain a powdery precursor; The powdered precursor is sintered to obtain a finished lithium iron phosphate positive electrode material.
5. A method for preparing a lithium iron phosphate positive electrode material according to claim 4, It is characterized in that The lithium source is at least one of lithium carbonate and lithium hydroxide monohydrate, and the carbon source is at least one of glucose, sucrose, citric acid, polyethylene glycol, carbon nanotubes, graphene, and carbon black.
6. A method for preparing a lithium iron phosphate positive electrode material according to claim 4, It is characterized in that The total mass of the carbon source is 3-20% of the mass of the finished lithium iron phosphate positive electrode material.
7. A method for preparing a lithium iron phosphate positive electrode material according to claim 4, It is characterized in that The ball milling time is 2h-10h.
8. A method for preparing a lithium iron phosphate positive electrode material according to claim 4, It is characterized in that The sintering is a two-stage sintering, and the sintering method includes: First, nitrogen is introduced and air is exhausted; Next, the first stage of sintering is carried out: the temperature is raised to 300-500°C, nitrogen is always introduced during the sintering period, and the sintering is carried out for 4-6 hours; Then, the second stage of sintering is carried out: the temperature is raised to 600-850°C and sintered at this temperature for 6-10 hours; Finally, the mixture was cooled to room temperature under a nitrogen atmosphere, and the cooled product was ground and pulverized to obtain a finished lithium iron phosphate positive electrode material.
9. A lithium iron phosphate positive electrode material prepared by the method according to any one of claims 4 to 8.
10. A lithium ion battery comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, It is characterized in that The positive electrode sheet includes the lithium iron phosphate positive electrode material as claimed in claim 9.
Citation Information
Patent Citations
New process for preparing low-cost cell-grade iron phosphate material from basic iron acetate
CN102431988A
Method for preparing lithium iron phosphate from nano-scale iron phosphate
CN110316712A
Method for preparing high-compaction iron phosphate through agricultural monoammonium purification
CN118561248A
Lithium iron phosphate, preparation method therefor, and lithium-ion battery
US20230170481A1